Automotive Clearcoat Haze: DOI, Wave Bands, Gloss Criteria

2026-11-28 · Category: Technical Knowledge

🌐 This article was automatically translated from Chinese. Please refer to the original Chinese version if needed. · View original (Chinese)

Automotive clearcoat haze, DOI and gloss acceptance criteria

Automotive clearcoat haze (reflection haze) is the scattering of light within a few degrees on either side of the specular angle, which produces a milky halo around the reflected image and lowers its contrast; it is reported in haze units (HU) or log haze (LogHU) and is a separate optical quantity from specular gloss in GU, from the 0-100 Distinctness of Image (DOI) index, and from orange peel described by wavelength bands. A familiar dispute at handover is this: 60° gloss readings on basecoat and clearcoat match exactly, yet the flank reflection looks grey and soft. The cause sits in the haze layer, while most acceptance clauses only specify gloss and leave no criterion for haze or DOI. This article arranges verifiable criteria for automotive clearcoat haze across five layers: measurement geometry, wave-band decomposition, film formation, rework boundary and clause drafting.

1. Six conclusions to read first

  • Haze is not loss of gloss. A published instrument datasheet lists two panels sprayed with the same coating: 20° gloss of 87.2 GU and 89.0 GU differ by only 1.8 GU, while DOI moves from 97.1 down to 84.3 (a gap of 12.8), LogHaze from 32.5 up to 37.6 and peak reflectance RSpec from 88.2 GU down to 54.7 GU. Reading gloss alone misses the defect.
  • ASTM E430 defines the image index as DOI = 100 x (1 - H0.3), so scattering in the +/-0.3° bands around the specular angle sets image sharpness; the same standard integrates haze for the 20° geometry from the 17°-19° and 21°-23° offset bands. Different angle conventions produce numbers that cannot be quoted interchangeably.
  • Where no goniophotometer is available, ASTM D4039 approximates reflection haze from two gloss readings: haze index H = G60 - G20, with G60 and G20 measured to the ASTM D523 geometry, which suits incoming-material and in-line screening.
  • ISO 2813 sets explicit angle thresholds: switch to 20° above roughly 70 GU at 60° for better discrimination, and to 85° below roughly 10 GU; a comparison series must keep one geometry, otherwise the difference contains an instrument term.
  • The Chinese method standard has been replaced: GB/T 9754-2025 Determination of gloss value at 20°, 60° and 85° for paints and varnishes was issued on 2025-06-30 and became effective on 2026-01-01, superseding GB/T 9754-2007 (identical to ISO 2813:1994, effective 2008-04-01).
  • Published industry guidance for mid- and high-grade passenger cars gives usable reference bands: 20° gloss no lower than 90 GU, DOI no lower than 80 on silver and 85 on dark shades, orange peel long wave no higher than 10 and short wave no higher than 20, PGD no lower than 0.8 on horizontal and 0.6 on vertical surfaces.

2. Where haze sits in the appearance chain

Light hitting a paint film splits into two paths. One keeps the specular direction and decides how bright the surface looks and how sharp the reflected image is. The other is absorbed, scattered and reflected several times inside the film and leaves in a near-diffuse way, deciding how clear the finish reads. Haze belongs to the second path but hugs the specular angle: it barely changes the total reflected flux, so the gloss meter stays flat, yet it consumes the contrast of the reflected image. Grouping haze, DOI and orange peel under "bad appearance" is an expensive mistake in both formulation talks and claim negotiations.

The scattering band lies a few degrees from the specular angle

Combined haze and gloss instruments first scan the full goniophotometric curve around the specular angle and then integrate the bands fixed by standard. On a 20° head, gloss is the composite within +/-0.9° of the specular angle (angle tolerance per ASTM D523 and ISO 2813), haze is the two bands 17°-19° and 21°-23° (angles per ASTM E430), and RSpec is the peak at +/-0.0991°. The instrument also sweeps 12.75°-27.25° to locate the specular angle, which compensates curvature and placement.

Reflection haze and transmitted haze are two conventions

Transparent sheet, headlamp lenses and heating films are usually quoted with ASTM D1003 transmitted haze together with luminous transmittance, which measures light that passes through the film and is scattered out; body clearcoat assessment measures light on the reflection side. The same film can give opposite conclusions under the two conventions: transmitted haze in spec while reflection haze out of spec means the defect is surface micro-structure rather than in-film phase separation. State which side you measured. Our separate article on transparent conductive heating coatings: sheet resistance, transmittance and haze trade-offs covers the transmitted convention; the two must not be mixed.

3. Measurement geometry and standard conventions

What each of the three angles is good for

The gloss unit is an artificial quantity: the polished black glass of refractive index 1.567 is defined as 100 GU, so the reading describes relative specular reflectance rather than flatness. The 20° geometry uses a smaller receiver aperture and concentrates resolution in the high-gloss range (about 70 GU at 60° and above), so clearcoats and metallic topcoats should be read at 20° first. The 85° geometry serves near-matt films below roughly 10 GU at 60° and separates matt and semi-matt clearcoats. The 60° geometry is the universal angle: it covers every film but does not separate two high-gloss panels. ISO 13803 specifies the 20° method and pairs with ISO 2813 as "universal angle plus high-gloss angle". Note that ISO 2813:1994 states the method is not suitable for the gloss of metallic paints, so metallic effect finishes need haze, DOI and flop measured together.

Offset angles and window widths make numbers non-transferable

ASTM E430 Method A uses a 20° fixed incidence and Method B a 30° one; only Method B carries DOI and 15° wide-angle haze. The window widths are fixed at 0.4° for the main specular band and 0.14° for the DOI sub-band (tolerance +/-0.01°), with narrow-angle haze offsets of +/-2° (28° and 32°). The standard requires a flat specimen of at least 70 mm, and Method B limits flatness deviation to 0.15°; a curved specimen depresses DOI directly. The calibration chain needs one high-gloss standard (polished black glass for non-metallic systems), one intermediate standard and one diffuse standard. These details mean that DOI and haze from different brands differ in the number itself while the ranking stays largely consistent, so a clause must reference a retained standard panel rather than a bare figure.

Table 1 Gloss, haze, DOI and orange peel: definition and measurement convention
Optical quantityQuestion it answersUnit and rangeStructure size it sensesTypical reference standard
Specular glossTotal reflected flux, that is how bright it looksGU; 20°, 60° and 85° geometriesOverall smoothness; insensitive below 0.1 mmISO 2813, ISO 13803, ASTM D523, GB/T 9754-2025
Reflection hazeScattering beside the specular angle, that is the milky veilHU or LogHU; LogH commonly 0-500 logHUMicro-structure below 0.1 mm and in-film phase separationASTM E430, ASTM D4039
Digital DOISharpness of the reflected image, that is mirror usefulness0-100, where 100 is an undistorted imageStructures near the eye limit, 0.1-0.3 mmASTM E430 Method B, ASTM D5767
Orange peel (waves)Wavelength distribution of the undulationBand scores Wa-We, du, SW/LWThe full 0.1-30 mm spectrumwave-scan type instruments, eye resolution experience

4. Short wave and long wave: mapping readings to process steps

A wave-scan instrument illuminates the surface with a point source at 60°, samples reflected intensity point by point and splits the optical profile with filter functions into bands: du below 0.1 mm, Wa 0.1-0.3 mm, Wb 0.3-1 mm, Wc 1-3 mm, Wd 3-10 mm and We 10-30 mm; the classical convention reports only SW 0.3-1.2 mm and LW 1.2-12 mm. The split matters because eye resolution depends on viewing distance: at about 3 m the eye best resolves structures of 10-20 mm, at about 40 cm it best resolves short waves of 1-3 mm and can resolve down to roughly 0.1 mm; structures finer than 0.1 mm no longer appear as light and dark bands but as a loss of clarity, which is exactly the territory of haze and DOI and explains why panels pass on Wd and We yet still look cloudy.

Substrate and sanding marks land on short wave, levelling and film thickness on long wave

Published instrument application notes give three reproducible attribution rules. First, on a horizontally sprayed panel the rougher the substrate, the worse the short-wave score, while long wave and DOI move little, which points to sanding marks and filler scratches. Second, moving from a horizontal to a vertical face worsens long wave while short wave and DOI stay nearly unchanged, which points to insufficient flash-off and levelling time as a precursor of sagging. Third, a thin clearcoat worsens long wave and building thickness lowers the long-wave score, a relationship with the time the surface keeps flowing rather than with the formulation. These three rules compress "bad appearance" into a specific process step and pair well with our article on film-thickness management for e-coat, primer, basecoat and clearcoat.

Table 2 Bands versus haze attribution: where the reading lands is where the responsibility lies
Reading bandWavelength rangeTypical causeShop-floor countermeasure
du micro-roughnessbelow 0.1 mmPoor resin compatibility, fine pigment or additive agglomerates, scattering from micro-bubbles after skin-overRecheck grind fineness and filtration, rebalance slow solvents, avoid early surface set
Wa + Wb (main DOI contributors)0.1-1 mmInsufficient levelling, short flash-off, coarse atomisationExtend flash and levelling, retune gun pass and pressure to panel temperature, control thickness uniformity
SW short wave0.3-1.2 mmSubstrate roughness, sanding marks, printed-through filler scratchesRaise mid-coat filling and sanding grade, seal the substrate before topcoat
LW long wave1.2-12 mmSag precursor on vertical faces, thin film, too fast bake rampBuild to the designed range, slow the ramp, split into passes
Wd + We ripples3-30 mmRobot trajectory, bell cup pass rhythm, fixture shieldingRecheck overlap and fan width, correct rhythm and part attitude

One caveat: the atomisation energy of a rotational bell differs from air spray, and published technical exchange material consistently reports higher HAZE from bell application than from air spray of the same formulation, so criteria must be re-based on a retained panel whenever the process changes. The correlation between orange peel and DOI is developed in our separate articles orange peel and distinctness of image control and the causes of orange peel texture, which are not repeated here.

5. Key data: acceptance must rest on numbers with units

  • Gloss: calibrated so that black glass of refractive index 1.567 equals 100 GU; read high-gloss clearcoats above roughly 70 GU at 60° at 20°, and matt clearcoats below roughly 10 GU at 85°, following the ISO 2813 angle convention.
  • DOI: per ASTM E430 Method B, DOI = 100 x (1 - H0.3) on a 0-100 scale; the DOI sub-window is 0.14° +/-0.01° and the main specular window 0.4° +/-0.01°.
  • Specimen geometry: ASTM E430 requires a specimen of at least 70 mm and flatness deviation no greater than 0.15°; wave-scan tools accept curvature radius above 500 mm, a specimen no smaller than 35 mm x 150 mm, scan lengths of 5, 10 or 20 cm and a resolution of 375 points per cm.
  • Instrument tolerance (published datasheet figures): haze resolution 0.1 HU, repeatability +/-0.5 HU, reproducibility +/-1.5 HU; log haze range 0-500 logHU with repeatability +/-1 logHU and reproducibility +/-10 logHU; 20° gloss resolution 0.1 GU, repeatability 0.2 GU, reproducibility 0.5 GU.
  • Eye anchors: 10-20 mm structures at about 3 m, 1-3 mm structures at about 40 cm with a limit near 0.1 mm; this difference is why ripples are checked from afar and haze up close.
  • Industry reference bands: 20° gloss at least 90 GU, DOI at least 80 on silver and 85 on dark, long wave no more than 10 and short wave no more than 20, PGD at least 0.8 horizontal and 0.6 vertical, and fullness judged favourably once the composite film reaches 110 μm.
  • Environment limits: do not spray above roughly 65% relative humidity, or when the dew point is within 20 °F (about 11 °C) of ambient; solvent evaporation can cool the film surface by as much as 20 °F (about 11 °C), which is the trigger for blushing haze.
  • Temperature and rhythm: the practical control point for two-component clear systems is 75 °F (about 24 °C) for storage and spraying, and at 20 °C a two-component clearcoat needs roughly 7 days to reach the hardness required before polishing.

6. Film formation: solvent gradient, skin-over and moisture condensation

During the tens of minutes between wet film and solid film three things run at once: an evaporation gradient builds through the film thickness, resin concentration rises so that viscosity climbs steeply, and shrinkage lets surface tension draw the surface into a mirror. Haze is the visible result whenever one of these three falls out of step. A too-fast solvent blend removes surface mobility before levelling completes and freezes the micro-structure in place; viscosity that is too high prevents atomised droplets from coalescing and leaves 0.1-0.3 mm micro-roughness; poor resin or additive compatibility, or additive migration, leaves refractive-index mismatches inside the film. The last type is invisible on a gloss meter and shows only on haze and RSpec.

Blushing haze: dew-point spread beats relative humidity

Spraying in humid conditions lets atomising air and evaporating solvent carry heat away together, dropping the wet film below the dew point so that water condenses into micro-droplets inside it and cures into a milky veil. Two criteria from refinish technical notices and shop practice can go straight into a work instruction: do not spray above roughly 65% relative humidity, and do not spray when the dew point is within 20 °F (about 11 °C) of ambient temperature. Because evaporating cooling can reach 20 °F (about 11 °C), a panel at room temperature is not automatically warm enough above the dew point. Fresh blushing can be driven off with heat or a light recoat containing retarder; light blushing on a cured film may be recovered by polishing, while heavy blushing needs sanding and re-spraying.

Bake ramp and the levelling window

A ramp that is too fast locks the surface before levelling finishes and worsens both long wave and haze; one that is too slow raises sag risk and also worsens long wave. The controllable quantity is how long the wet film stays mobile, set by the combination of reducer grade, per-pass thickness and flash time. Refinish reducers are commonly banded by temperature: fast below 70 °F (about 21 °C), medium between 70 and 80 °F (about 21-27 °C), slow above 85 °F (about 29 °C). Using a fast reducer in a 90 °F (about 32 °C) booth causes dry spray, the opposite end of the same mechanism.

7. How formulation and process parameters map onto haze readings

Treat haze as the response variable and the drivers can be ranked by contribution. The ranking follows the primary and secondary cause split in published technical exchange material and instrument application notes: the coating itself (pigment dispersion state, additive type, resin compatibility) is the primary group, while substrate roughness, flatness, sanding marks and application method are secondary.

  • Pigment and extender dispersion: incomplete grind or thickening in storage creates 0.1 mm scattering centres; verify with a grind gauge and filtration residue rather than with a gloss meter.
  • Resin and solvent compatibility: a reducer with too little solvency generates local gel particles, which on a clear coat reads as an even grey veil instead of patches.
  • Additive migration and compatibility: excess levelling agent or a narrowing compatibility window precipitates micro-phases during cure; matt systems also carry matting agent settling, developed in matt gloss stability and matting agent settling.
  • Application method: bell cup and air spray have different atomisation energy and therefore different haze baselines, so cross-process quoting requires a new retained panel.
  • Film thickness and uniformity: a thin coat worsens long wave while a thick one extends levelling but adds sag risk; see film-thickness management.
  • Cleanliness and dirt: particles raise short wave and haze on their own; controls are in dirt inclusion and cleanliness control for automotive paint.
  • Body geometry: roping lines and press lines on aluminium outer panels turn haze into directional streaks, so judge together with the car paint defect checklist.

Instrumental inspection of vehicle paint and coating condition for haze assessment

8. Rework boundary: how far polishing can rescue a panel

The boundary for haze rework is not a feeling but the depth of the scattering source. When scattering lives only in the clear surface (polishing traces, slight early-cure micro-roughness, light blushing), removing a few tens of micrometres restores the image. When it comes from inside the film (compatibility precipitates, bubbles, pigment agglomerates, printed-through substrate), polishing only thins the coat and worsens the edge. A usable criterion: record 20° gloss, LogHU and DOI at one position, run a small test polish, then continue only if DOI rises while LogHU falls and RSpec rises clearly, which shows surface-level scattering. If DOI and RSpec do not move while gloss drops, the film is entering the burn-through zone and the panel should go to re-spray.

Quantified preconditions for a polish rescue

At 20 °C a two-component clearcoat needs roughly 7 days to reach its final polishing hardness; polishing earlier converts haze from an in-film defect into a mechanical one and leaves rotation marks and holograms. The published sequence is progressive grit refinement (for example 2000 grit followed by 3000 grit) with generous wet sanding, then machine polishing with a medium cutting compound and a foam pad in the 1200-1800 rpm band; these figures come from refinish supplier material and are practical guidance, so a production line should calibrate against its own retained panel. Grit staging and anti-mark technique are detailed in wet sanding and polishing of automotive paint.

Three cases that require re-spray

First, in-film blushing that survives heat and recoating, meaning moisture is sealed inside. Second, DOI and RSpec both low with no movement after polishing, meaning the micro-structure sits at an interface rather than the surface. Third, short wave repeating the substrate pattern, which is printed-through sanding marks and cannot be polished away, only hidden. In those cases return to mid-coat and substrate work, and first rule out weathering-related gloss loss with the distinction between clearcoat gloss loss and yellowing, so that chemical loss of gloss is not treated as haze rework.

9. Drafting the acceptance clause

An executable clearcoat appearance clause locks six items at once: measurement geometry (angle and instrument standard), the reference (a retained panel rather than a bare number), the judgment positions and point counts (horizontal and vertical faces separated), the environment (panel temperature, ambient temperature, relative humidity or dew-point spread), the state (wet film, tack free, fully cured) and the tolerance (difference versus the retained panel rather than a bare figure). Drop any one and the reading gap between supplier and buyer becomes a commercial dispute. The table below lists common criteria with units and binding conditions, ready to be rewritten as a contract annex.

Table 3 Acceptance criteria for clearcoat appearance: values, units and binding conditions
CriterionUnit and rangeReference valueConditions that must be bound
20° glossGUIndustry reference no lower than 90Geometry, black glass calibration, same instrument or a cross-check factor
Reflection hazeHU or logHUDifference versus the retained panel inside instrument reproducibility (commonly +/-1.5 HU or +/-10 logHU)Offset-angle convention and whether colour-compensated haze is used
DOI0-100At least 80 on silver, at least 85 on dark shadesMethod A or B, curvature radius above 500 mm, flatness deviation no greater than 0.15°
Orange peel SW / LWBand scoreIndustry reference short wave no more than 20, long wave no more than 10Instrument model and scale (SW/LW or Wa-We), scan length
PGD0-1At least 0.8 horizontal, at least 0.6 verticalReference image and viewing distance, lighting condition
Composite film thicknessμmIndustry reference at least 110Measurement positions, dry or wet film, substrate material

Judging environment: three light sources, three verdicts

Handover areas usually combine daylight, a light booth and shop ceiling lighting. The practical convention is: check ripples and long wave under distant diffuse light, check haze and DOI under a nearby point source, and check whether the highlight edge is crisp by oblique reflection. Metallic finishes depend heavily on the reflected image itself, so use the same light source and viewing distance for every record and state the light type in the report. Colour batching inside a standard light booth is not the same as appearance judging: the first controls colour difference, the second controls scattering. The photograph below shows the common laboratory scene of comparing coating appearance and colour under standard light.

Coating colour and appearance comparison under standard light source, environment consistency for haze judging

Wet film, tack free and fully cured readings differ

In the wet stage surface tension is still working, so haze and DOI usually read better than the final result; once the resin network has shrunk and cure completes, the micro-structure is locked. The clause should state how many hours after cure the judgment is made, otherwise the supplier quotes the off-line reading and the buyer re-measures after 7 days and both are correct. Matt and semi-matt clearcoats must additionally bind the angle choice: judging a matt film only at 60° averages away the directional difference caused by matting agent settling, a misjudgement developed further in matting agent settling and gloss stability.

Reflected image and highlight edge on a metallic automotive finish, visual expression of haze and DOI

10. Frequently asked questions

Q1. Gloss passes but the customer says the panel looks hazy. How do we show the coating is not at fault?

Add two measurements at the same position: reflection haze (HU or logHU) and DOI at 20° or 60°, and record RSpec. If gloss is inside tolerance while LogHU is above the retained panel, DOI is below it and RSpec is clearly below the gloss value, the defect is real and of the scattering type, which does not contradict a passing gloss reading. If all three match the retained panel, the difference most likely lies in the observation condition (light source, distance, angle) rather than in the coating, and the report should list the three readings together with the viewing conditions.

Q2. Should haze be reported as linear HU or as LogHU, and are they convertible?

Both scales exist on mainstream instruments. The logarithmic scale is more common on paints and clearcoats because it tracks human perception of haze more closely; linear HU and LogHU are two mappings of one physical quantity and the mapping is defined by the instrument, so converting between brands is not advisable. A clause should state the standard convention plus the difference versus the retained panel and prescribe repeatability and reproducibility, for example the common +/-0.5 HU repeatability and +/-1.5 HU reproducibility for haze, because a gap smaller than reproducibility is not evidence of a process difference.

Q3. Why do metallic paints need compensated haze?

On non-metallic films the diffuse component follows Lambert's law closely, so the brightness channel can subtract diffuse reflection. On metallic and effect pigments the reflection is directional and almost nothing returns at the brightness angle, so conventional haze reads systematically high. Metallic parts therefore need a head with directional reflection compensation, or a shorter collection distance metric such as RIQ, and the clause should record whether colour compensation was applied, otherwise batch-to-batch comparison on the same colour loses validity.

Q4. DOI is low while the orange peel reading is normal. What can that be?

DOI responds mainly to structures below 0.1 mm and correlates most tightly with du, Wa and Wb. A normal SW and LW score only says the 0.3-12 mm range is acceptable. Check du, Wa and Wb next, then in-film scattering (compatibility, micro-gel, additive precipitation) and surface residue (polishing marks, release agent transfer). This is precisely why orange peel passing does not imply a sharp image, and why the two need separate limits.

Q5. Two instruments differ by 8 DOI points on the same panel. Is that the equipment or the paint?

Check the geometry first. ASTM E430 Method A and Method B use different specular angles (20° and 30°) with different window widths and offset bands, and manufacturers add their own DOI fitting functions, so the two sides cannot be compared directly. The practical route is a correlation test on one retained panel across both heads, producing a conversion factor and a confidence interval, with acceptance written as the difference versus the retained panel. Only when both heads are stable on the retained panel and the film DOI scatter exceeds reproducibility should the cause be assigned to the process.

Q6. How should humidity and dew point enter a work instruction?

Write two hard thresholds: no spraying above roughly 65% relative humidity, and no spraying when the dew point is within 20 °F (about 11 °C) of the panel. Also require a measured panel temperature instead of a quoted room temperature, because evaporative cooling can lower the film surface by up to about 20 °F (about 11 °C). In humid conditions add the retarder amount recommended by the supplier, reduce thickness per pass and extend the interval between passes, which stops blushing haze before the film sets.

Q7. Where is the boundary for a rework polish, so polishing does not create more haze?

Use three lines: full cure as a precondition (about 7 days at 20 °C), the reading change after a local test polish (continue only when DOI rises and RSpec rises), and the remaining dry film thickness (the removal must stay inside the designed thickness allowance). If a test polish leaves DOI and RSpec unchanged while 20° gloss falls, the film has entered the burn-through zone: stop polishing, re-spray, and re-check the remaining thickness against the film-thickness control document.

11. References and basis of the figures

  • ASTM E430, current edition E430-23, for measurement of gloss of high-gloss surfaces by abridged goniophotometry: Method A at 20° incidence and Method B at 30°, DOI = 100 x (1 - H0.3), receiver window widths, offset bands, a specimen of at least 70 mm and flatness deviation of 0.15° are all taken from that text.
  • ASTM D4039 (D4039-09, reaffirmed 2023) for reflection haze of high-gloss surfaces from two gloss readings, with references to ASTM D523, D3964, D823, E284 and E430, classified under ICS 87.040.
  • ISO 2813, whose 1994 edition (EN ISO 2813:1999 withdrawn on 2014-11-07) was retitled in 2014 as determination of gloss value at 20°, 60° and 85°: 20° for films above roughly 70 GU at 60°, 85° for films below roughly 10 GU, and the 1994 text states the method is unsuitable for metallic paints.
  • ISO 13803:2014 for 20° gloss of paint films, and GB/T 9754-2025 (issued 2025-06-30, effective 2026-01-01, superseding GB/T 9754-2007), administered by the National Standardization Technical Committee of Paints and Coatings (SAC/TC5).
  • The wave-scan band definitions (du, Wa-We, SW/LW), the eye resolution anchors, the specimen size of 35 mm x 150 mm and the curvature radius above 500 mm come from published instrument manufacturer material and application manuals.
  • The automotive appearance criteria (20° gloss, DOI, long and short wave, PGD, composite thickness) and the observation that bell application gives higher HAZE than air spray come from public technical exchange material issued by a coatings company in 2023 and from industry compilations; they are practical reference bands, not mandatory clauses.
  • The humidity and dew-point criteria for blushing, the retarder countermeasure and the polishing recovery boundary come from refinish technical notices and public application material, again as field experience; confirm the figures against the technical data sheet of the system in use.
  • All standards and figures here are compiled and interpreted from public sources; formal judgments must follow the current standard text and the retained panel agreed between supplier and buyer. Kexin supplies on a business-to-business basis with EXW and FOB as the trade terms.

Last updated: 2026-11-28 | Kexin New Materials (Guangdong) Co., Ltd. · Kexin New Materials (Guangdong) Co., Ltd. B2B technical support for automotive OEM and refinish coating, supply terms EXW / FOB, including haze and DOI panel comparison programmes, application window parameter sheets and small-batch trial panel validation.

Tags: #Automotive coatings #Automotive Coatings #Coatings technology literature