Reinforced concrete anti-corrosion is the coordinated protection of a reinforced concrete structure around one goal: keeping chloride ions and moisture away from the rebar so its passive layer survives. It combines a dense concrete body with adequate cover depth, a corrosion-inhibiting primer that maintains passivation at the steel interface, and a surface system — silane impregnation or a film-forming coating — that cuts off the external supply. Only the three lines working together can push rust-induced cracking beyond the design life.
Failure usually starts in an unremarkable spot. On the high-pile beam-and-slab deck of a seaport wharf in northern China, after 18 years of service the soffits of splash-zone beams were the first to show flexural cracks 0.3~1.2 mm wide running along the rebar; half-cell potentials read -385 mV (CSE), and cores taken through the cover showed acid-soluble chloride at 0.9% of cement mass — far beyond the 0.4% depassivation threshold. When the cover was broken out, millimeter-thick rust scales peeled off the bars: the 2~6-fold volumetric expansion of the corrosion products had long since jacked the concrete apart along the bars. Chloride does not corrode concrete; it corrodes the steel inside it, and the window for economical repair closes before the cracks appear.
TL;DR: six coordinated criteria for reinforced concrete anti-corrosion
- Threshold: depassivation begins when acid-soluble chloride at the rebar surface reaches roughly 0.4% of cement mass (ASTM C1152 titration basis); a [Cl⁻]/[OH⁻] molar ratio above 0.6 is the other common yardstick. Carbonation lowers the threshold to about 0.2% once pH drops from roughly 12.5 to below 11.5.
- Potential: the three ASTM C876 half-cell bands on a CSE scale — above -200 mV, low corrosion probability; -200~-350 mV, uncertain, densify the survey; below -350 mV, high probability, start repair assessment.
- Density: by ASTM C1202, 100~1000 C counts as "very low" chloride permeability and above 4000 C as "high" (60 V, 6 h); marine-grade concrete measured by the GB/T 50082-2009 RCM method typically lands in the 4.5~5.5×10⁻¹² m²/s class (published-data basis).
- Inhibition: calcium nitrite is commonly dosed at 2~3 kg/m³ in new mixes, while migrating amino-alcohol products need an effective local concentration at the rebar (about ≥2.0 kg/m³, published-data basis). Both are auxiliary lines and never a substitute for concrete quality.
- Coating: EN 1504-2 requires an equivalent air-layer thickness Sd,CO2 ≥50 m against CO₂ and pull-off adhesion ≥1.0 N/mm²; silane impregnation totals 0.4 kg/m² in two passes with acceptance at ≥85% water-absorption reduction and ≥90% chloride-uptake reduction (JTJ 275-2000 basis).
- Source control: GB 50164-2011 caps water-soluble chloride in the fresh mix at ≤0.3% of binder for class-I environments, ≤0.2% for class II, ≤0.1% for severe classes, and ≤0.06% for prestressed members.
Mechanism: how chloride breaks the passive film on rebar
Pore solution in fresh concrete sits at pH 12.5~13.5, and in this strongly alkaline environment the steel spontaneously grows a dense passive film a few nanometers thick — the steel is "protected" by the concrete, not by its own composition. Anti-corrosion therefore reduces to two tasks: keep that alkaline reserve intact (carbonation control) and keep chloride from reaching the steel surface (chloride control). Lose either one and the film destabilizes locally, forming a "large-cathode, small-anode" pitting cell that eats downward rather than spreading evenly — which is why hairline rust cracking along bars is so hard to catch by eye in its early stage.
Transport paths: diffusion, capillary suction and pressure penetration
Chloride reaches the steel through three routes. Diffusion dominates: where surface and internal concentrations differ, ions migrate through pore water toward the depth, and the lower the water-binder ratio and the richer the SCMs, the narrower this channel. Capillary suction is the fiercest in wetting-drying zones: a dried surface develops pore negative pressure, and the next brine contact sucks solution into the surface layer, so splash and tidal zones accumulate chloride far faster than submerged zones. Pressure penetration matters where the water head is high (retaining walls, caisson faces), pushing ions through connected pores in bulk. The three routes stack, so one mix can show order-of-magnitude lifetime differences between exposure zones. Chloride is not the only threat to concrete; see biogenic sulfuric acid corrosion of sewer concrete for the acid route.
Critical concentration: 0.4% and [Cl⁻]/[OH⁻] above 0.6
Engineering uses two yardsticks for "when rust starts". One is total acid-soluble chloride as a percentage of cement mass: published sources place the risk band at 0.2%~0.4%, with roughly 0.4% the typical depassivation trigger (ASTM C1152 titration basis). The other is the [Cl⁻]/[OH⁻] molar ratio in pore solution: above 0.6 pitting risk rises sharply, and calcium-nitrite inhibitors also lose effectiveness beyond that ratio. Carbonation pushes both thresholds down: once pH falls below 11.5, bound chloride re-releases as free chloride and the critical value drops to about 0.2% — which is why "carbonation plus chloride" is far harsher than either factor alone. Table 1 summarizes the criteria.
Dense body: mix design and cover are the capital
How wide those channels run depends on the capital the concrete body provides. Water-binder ratio is the primary variable: above 0.45, capillary porosity climbs visibly and the diffusion channel widens. SCMs are the second: fly ash and slag consume calcium hydroxide and refine pore structure, silica fume plugs nano-scale pores, and published data show mixes with 30% fly ash or slag cutting D_RCM roughly in half, with 8%~10% silica fume performing even better. Cover depth is the third: diffusion time scales roughly with the square of cover, and GB 50010-2010 and GB/T 50476-2019 set class-dependent minimums, with splash-zone members commonly built at the 60 mm level in industry practice (published-data basis). Cracks are the leak in that capital: a 0.1 mm-wide crack raises chloride ingress 3~5-fold against sound areas (published-data basis), so even a superb mix relies on crack control to deliver. Where the body is poor, the outer two lines only extend life — they cannot save the structure.
Field assessment: potential, chloride profile and density testing
Assess before you protect. The survey answers three questions: has corrosion started (potential), where has chloride reached (profile), and how much capital is left in the body (density). Only the three datasets together decide whether the job is "protective strengthening" or "repair plus protection".
Three-band half-cell criteria (ASTM C876)
The half-cell potential method grids a copper/copper-sulfate reference electrode (CSE) over a moist surface: the more negative the reading, the higher the depassivation probability. The classic ASTM C876 bands: above -200 mV, corrosion probability below 10%, re-survey on the normal cycle; -200~-350 mV, uncertain band, densify the grid and open inspection holes; below -350 mV, probability above 90%, lay out breakout repair and protection assessment. Readings are moisture-sensitive — dry patches shift positive — so keep the surface wet and log ambient conditions.
Chloride profile and diffusion coefficient (coulomb and RCM)
Core through suspect areas and slice by depth (for example 0~25 mm and 25~50 mm layers) for acid-soluble titration; plotting chloride versus depth against the 0.4% line shows how far the chloride peak sits from the steel. For density, ASTM C1202 passes 60 V DC for 6 h and records coulombs: 100~1000 C is "very low", 1000~2000 C "low", 2000~4000 C "moderate", above 4000 C "high". Chinese practice prefers the GB/T 50082-2009 rapid chloride migration (RCM) coefficient D_RCM in 10⁻¹² m²/s units for durability design. Mixes with 30% fly ash or slag commonly halve D_RCM (published-data basis, see the note under Table 1). The two tests do not convert into each other: coulomb results understate silica-fume mixes, so run whichever the contract names.
| Assessment axis | Method / basis | Criteria | Engineering action |
|---|---|---|---|
| Corrosion initiation | ASTM C876 half-cell potential (CSE) | Above -200 mV low; -200~-350 mV uncertain; below -350 mV high | Plan breakout repair and protection assessment in high-risk zones |
| Corrosion rate | Linear polarization resistance (published-data basis) | i_corr above 0.5 µA/cm² high; 0.1~0.5 µA/cm² moderate; below 0.1 µA/cm² low | Cross-check section loss for capacity and repair priority |
| Chloride depth | Core slicing with acid-soluble titration (ASTM C1152) | Chloride peak approaching 0.4% of cement mass near the rebar | Start inhibition plus surface protection; shorten the re-survey cycle |
| Body density | ASTM C1202 coulomb / GB/T 50082-2009 RCM | 100~1000 C "very low"; above 4000 C "high" | Reinforce with coating and impregnation where density falls short |
Corrosion-inhibiting primer: migrating versus non-migrating chemistry
Inhibitors are the line that "keeps passivation alive" at the steel interface. Two supply routes exist: inhibitors mixed into fresh concrete, and coating-type inhibiting primers brushed or sprayed onto rebar or concrete surfaces during repair. Neither changes concrete density nor replaces a coating barrier; their role is to make arriving chloride harmless. For the nano-composite filler route in metal protection, see nano-composite anti-rust fillers: barrier, inhibition and synergy.

Non-migrating: anodic passivation by calcium nitrite
Calcium nitrite is the classic anodic inhibitor: nitrite re-oxidizes freshly formed ferrous ions back to stable passivity, effectively patching the pit bottom. Its limit is equally explicit — once chloride loading is high ([Cl⁻]/[OH⁻] above 0.6) the nitrite resupply cannot keep pace with consumption and protection decays, so dosage must scale with the chloride load. Published sources place common reinforced-concrete dosage at the 2~3 kg/m³ level, with exact dosing set per JGJ/T 225-2010 (Chinese technical specification for corrosion inhibitors) and manufacturer chloride-matching trials. Nitrites are restricted for prestressed and potable-water-contact structures, so check the codes before selecting.
Migrating: film formation by amino alcohols
Migrating corrosion inhibitors (MCI) are small amino-alcohol molecules that diffuse along pore liquid and vapor phases from the concrete surface toward the rebar, adsorbing as monolayers on both cathodic and anodic sites. Their advantage is retrofit: for structures already penetrated by chloride but not yet corroding, surface application or flood-grouting onto the surface layer starts work immediately; published sources put the effective local concentration at roughly ≥2.0 kg/m³ with penetration to the 30 mm class. Effectiveness depends heavily on applied quantity and coverage uniformity, and acceptance reads as a positive potential shift (≥100 mV, published-data basis) with reduced corrosion current.
Inhibiting primer ≠ zinc-rich primer: keep the functions apart
Repair crews often confuse the two. Zinc-rich primers protect bare steel through galvanic sacrificial action plus barrier effect — the right choice for exposed steelwork. In reinforced-concrete repair, the rebar is re-embedded in mortar and protected by maintained passivity, so the correct choice is an epoxy inhibiting primer (dry film at the ≥100 µm class, published-data basis) or a migrating inhibitor, letting the mortar and the inhibition function chain up, rather than sealing zinc inside mortar. Table 2 compares the three routes.
| Route | Mechanism | Typical dosage | Fits / limits |
|---|---|---|---|
| Mixed calcium nitrite | Anodic passivation; patches pit bottoms | 2~3 kg/m³ (scaled with chloride load) | New mixes; restricted for prestressed and potable-water contact |
| Migrating amino alcohol (MCI) | Vapor/liquid diffusion adsorption; dual anode-cathode suppression | Surface coat/grout; ≥2.0 kg/m³ local effective concentration | Existing structures; depends on applied quantity and uniformity |
| Coating epoxy inhibiting primer | Physical barrier plus inhibiting pigment | Dry film ≥100 µm | After breakout before mortar; must pair with mortar system |
Coating synergy: sealing, shielding and anti-carbonation roles
The surface line "cuts off supply": keep chloride and CO₂ out while letting internal vapor escape. Three routes divide the work — silane impregnation makes pore walls hydrophobic, film-forming coatings shield the whole surface, and crystalline systems plug capillaries. For system-level selection see concrete protective coating systems: penetrating, film-forming and reactive strategies.

Silane impregnation: hydrophobic but not sealing
Isobutyl triethoxysilane penetrates the surface capillaries and condenses with wall hydroxyls, pushing the contact angle to the hydrophobic side: liquid water and dissolved chloride cannot enter, water vapor still escapes, and pores stay open. Practice applies two airless passes on a surface aged 28 d and dried to ≤6% moisture, totaling 0.4 kg/m² (first pass 0.25 kg/m², second 0.15 kg/m², about 6 h apart). The JTJ 275-2000 acceptance basis is ≥85% reduction in water absorption and ≥90% reduction in chloride uptake, with impregnation depth verified by core slicing. Silane carries no mechanical shielding, so abraded or scoured areas need a film-forming coat on top.
Epoxy sealer plus topcoat: the film-shield package
Film systems run a "sealing primer plus topcoat" two-layer build: the primer blocks surface capillaries and restores a paintable face, the topcoat adds weathering resistance and shielding. Concrete is strongly alkaline, so the primer must resist saponification — selection logic in sealing primers and alkali-resistant topcoats for concrete; choose a weathering topcoat (aliphatic polyurethane or fluorocarbon), and where steelwork is painted on the same site, unify film management per general anti-corrosion systems for steel structures. EN 1504-2 sets two hard numbers: equivalent air-layer thickness against CO₂, Sd,CO2 ≥50 m, and pull-off adhesion ≥1.0 N/mm²; it also requires water-vapor permeability Sd ≤5 m (class I) so the film "breathes" — trapping vapor moves delamination risk to the inside face of the coating.
Film shielding lives or dies on distribution, not nominal thickness. Published sources put total dry film for concrete protection at the 250~500 µm class: 50~100 µm of primer for sealing, 100~150 µm of topcoat for weathering. Watch three items in the field: substrate moisture (most products demand ≤8%) and age; spot layout of one reading per 10 m² with ≥90% acceptance (published-data basis); and edges, bolt holes and cracks, which are thin-film weak points needing stripe coats. Film management rhymes with e-coat rack logic — uniformity predicts life better than the average.
Anti-carbonation and breathability: the paired EN 1504-2 constraints
Carbonation does not rust steel directly; it dilutes the alkaline reserve the passive film depends on, and stacked with chloride it becomes a double strike. The quantitative language for an anti-carbonation coating is Sd,CO2 — the thicker the equivalent air layer, the slower CO₂ crosses; in EN 1062-7 grading only values ≥50 m count as effective. Yet "thick" and "tight" are not synonyms: coatings with too low a vapor-permeability class blister and peel on moisture-cycling walls, which is why EN 1504-2 pairs Sd,CO2 ≥50 m with Sd ≤5 m (class I breathability). Both numbers belong in the report, not just film thickness. Table 3 summarizes the three systems.
| System | Key dosage / criteria | Strengths | Limits |
|---|---|---|---|
| Silane impregnation | 0.4 kg/m² total (0.25+0.15); absorption reduction ≥85%, chloride-uptake reduction ≥90% | Breathable, invisible finish, fast application | No mechanical shielding; needs a film coat in wear zones |
| Epoxy sealer plus polyurethane/fluorocarbon topcoat | Sd,CO2 ≥50 m; adhesion ≥1.0 N/mm²; Sd ≤5 m | Controllable shielding and anti-carbonation, colorable | Depends on surface preparation and film management |
| Cement-based crystalline coating | About 1.5 kg/m² (published-data basis) | Self-seals microcracks below 0.4 mm | Limited chloride barrier; cannot deliver a decorative face |
Repair: breakout boundaries, interface work and re-protection
Repair in chloride environments is not "smooth it over". Break out beyond the weak zones flagged by potential and chloride profile — typically 50 mm past the boundary and beyond the ends of rust cracks — expose the bars, mechanically descale to near-bright metal, apply an inhibiting primer or migrating inhibitor, reinstate with low-chloride polymer-modified mortar, then re-protect the whole surface. Patching only the breakout area without re-protection turns the new-old interface into the next chloride entrance.
The interface decides whether the patch "grows onto" the old structure. Roughen the breakout face to expose sound substrate, clean dust with high-pressure water or air, apply a bonding agent, and fill polymer mortar in compacted layers (published sources keep single layers near 20 mm); verify bond at the joint by pull-off (commonly ≥1.5 MPa, published-data basis). Choose low-chloride, low-shrinkage mortar: chloride carry-in eats the inhibitor reserve, and excess shrinkage pulls fresh microcracks along the interface. After the mortar cures and moisture drops into range, re-apply the whole protection system per the coating section — order matters.
Disposition follows rebar section loss (published-data basis, Table 4): below 5%, surface treatment plus inhibition; 5%~15%, breakout repair with bond verification; above 15%, structural verification and, where needed, electrochemical protection. Impressed-current cathodic protection (ICCP) follows ISO 12696: current density 5~20 mA/m², protection potential held at -850~-1100 mV (CSE), with ≥100 mV depolarization over a 24 h off-break as the effectiveness criterion.
| Rebar section loss | Disposition route | Key actions |
|---|---|---|
| Below 5% | Surface treatment plus inhibition | Descale, inhibiting primer, local mortar patch, re-survey potential |
| 5%~15% | Breakout repair plus re-protection | Extended breakout, bonding agent, polymer mortar, full coating/impregnation |
| Above 15% | Structural verification plus strengthening or electrochemical protection | Capacity check, bond assessment, ICCP or member replacement |
Acceptance in synergy: quantitative criteria per defense line
Accept each line on its own numbers — "we applied it" is not "we applied it right". The core figures follow, each with units:
- Chloride threshold: 0.4% of cement mass at the rebar (ASTM C1152 titration basis) triggers depassivation; about 0.2% after carbonation; fresh-mix source control per GB 50164-2011 at ≤0.3% class I, ≤0.2% class II, ≤0.1% severe, ≤0.06% prestressed.
- Rust mechanics: corrosion products expand 2~6-fold, the direct driver of cover cracking; flexural cracks 0.3~1.2 mm wide usually signal active corrosion inside.
- Coulomb: ASTM C1202 six-hour values — 100~1000 C "very low", 2000~4000 C "moderate", above 4000 C "high" (60 V, 6 h).
- Diffusion coefficient: GB/T 50082-2009 RCM values D_RCM — marine standard mixes commonly 4.5~5.5×10⁻¹² m²/s, slag/fly-ash high-performance mixes about 1.8~2.8×10⁻¹² m²/s (published-data basis).
- Inhibitors: mixed calcium nitrite commonly 2~3 kg/m³; migrating products need ≥2.0 kg/m³ effective local concentration (published-data basis); effectiveness re-checked as potential shift ≥100 mV or corrosion current below 0.1 µA/cm².
- Silane impregnation: two passes totaling 0.4 kg/m² (0.25 kg/m²+0.15 kg/m², about 6 h apart), absorption reduction ≥85%, chloride-uptake reduction ≥90% (JTJ 275-2000 basis), depth verified by core slicing.
- Coating: EN 1504-2 pair — Sd,CO2 ≥50 m and adhesion ≥1.0 N/mm² (field pull-off per GB/T 5210/ISO 4624), vapor permeability Sd ≤5 m (class I).
- Cathodic protection: ISO 12696 basis — current density 5~20 mA/m², protection potential -850~-1100 mV (CSE), depolarization ≥100 mV over 24 h off-break.
For pull-off acceptance values and failure-mode grading, see adhesion acceptance for anti-corrosion coatings: pull-off values and failure modes.
Six common mistakes
- Treating the coating as the inhibitor: coatings cut external supply but cannot reach chloride already at the steel; when the peak nears the threshold, inhibit first, then protect.
- Silane with no film shield: silane breathes but carries no mechanical strength; traffic wear, scour and freeze-thaw zones need a film-forming coat on top, or the hydrophobic layer wears away and protection collapses.
- Trapping vapor: breathability (Sd ≤5 m) and anti-carbonation (Sd,CO2 ≥50 m) appear as a pair; picking thick film without testing vapor transport just moves blistering and peeling to the inside face.
- Repairing without a chloride profile: without the concentration curve you cannot judge how far the peak sits from the steel, breakout width becomes guesswork, and recurrence is near-certain.
- Inhibitors as a substitute for density: every inhibitor presumes the concrete body can hold; on a body above 4000 C coulombs, restore density before talking synergy.
- Accepting on film thickness alone: pull-off adhesion, vapor permeability, absorption reduction and potential re-survey are all acceptance items; miss any one and the synergy cannot close its loop.
FAQ: eight questions on reinforced concrete anti-corrosion
Concrete does not rust — why protect it at all?
The concrete body is indeed stable in most environments, but the engineering object is the composite system "reinforced concrete": steel stays inert in alkaline pore solution thanks to its passive film, and chloride plus carbonation dismantle that film from the chemical and electrochemical sides respectively. Once the film breaks, corrosion products expand 2~6-fold and jack the cover apart from inside, while moisture and chloride race in along the cracks — a self-reinforcing loop. Anti-corrosion is effectively renewing the passivation environment of the steel, and it costs far less than breakout repair after rust cracking, which is priced by area and carries downtime on top.
How is the 0.4% critical concentration actually used?
Treat it as a criterion, not a safety line: plot the chloride profile from core slicing, read the concentration at rebar depth against 0.4% of cement mass, and cross-check with the ASTM C876 potential bands. Concentration already past 0.4% while potential still above -200 mV means global depassivation has not set in — the protection window is still open; when both cross, treat it as active corrosion. In carbonated areas lower the yardstick to about 0.2%, and for prestressed members control the source at the GB 50164-2011 limit of 0.06%.
Can an inhibiting primer still help a structure with rust cracks?
Yes, but the role changes. Cracks mean corrosion is active, so the primer now works to "suppress further corrosion and support repair" rather than prevent initiation. The right sequence: delimit breakout by potential map and chloride profile with an extension, descale mechanically, apply the inhibiting primer or migrating inhibitor, reinstate polymer-modified mortar, then re-protect the whole surface with silane or a film system; areas above 15% section loss go to structural verification per Table 4. Coating over the crack without breakout only hides the process until spalling.
Silane impregnation or film-forming coating — which one?
Follow the zone and its dominant degradation. Atmospheric, carbonation-dominated elevations point straight at film coatings (Sd,CO2 ≥50 m) targeting CO₂; splash and tidal zones with wet-dry cycling and heavy salt supply get more direct relief from silane hydrophobic pore-wall modification, which tolerates wet faces. Wear, scour or decorative requirements call for film systems or a film coat over silane. The two are not mutually exclusive: heavily loaded areas commonly run "silane base plus film top", each line covering capillary ingress and overall shielding respectively.
Will the coating trap moisture inside?
It can — which is exactly why EN 1504-2 hard-codes breathability. Concrete moisture cycles with the seasons and vapor needs an outward path; a coating with too low a vapor-permeability class accumulates steam pressure at the coating-concrete interface, showing up as blistering and sheet peeling with concrete torn off the underside. Write both requirements into the specification — Sd ≤5 m (class I) alongside Sd,CO2 ≥50 m — and test each at acceptance; they cannot substitute for each other.
Do inhibitors affect concrete strength?
At compliant dosage the impact is manageable, but run compatibility trials. Calcium-nitrite products at common dosage (2~3 kg/m³, published-data basis) usually stay within test scatter for setting and strength; enlarged dosage or certain superplasticizer combinations can retard setting. Migrating types are surface-applied, never enter the mix, and have no direct strength effect. In practice run paste fluidity and strength comparisons per JGJ/T 225-2010, require a compressive-strength ratio of at least 95% (published-data basis), and fold chloride and alkali homogeneity into incoming inspection.
What gets measured at acceptance?
Accept line by line: for the body, coulomb (ASTM C1202, target the "very low" 100~1000 C class) or the RCM coefficient; for inhibition, re-survey half-cell potential (a ≥100 mV positive shift reads effective, published-data basis) and corrosion current; for silane, absorption reduction ≥85% and chloride-uptake reduction ≥90% with core-verified depth; for coatings, pull-off adhesion ≥1.0 N/mm² (GB/T 5210/ISO 4624), film thickness, plus Sd,CO2 and breathability class. Passing each item alone does not make the system pass — all four datasets belong in one acceptance record.
What does Kexin New Materials provide?
Kexin New Materials (Guangdong) Co., Ltd. serves industrial and engineering customers on reinforced concrete protection packages as a B2B supplier: selection advice covering sealing primers, inhibitor packages, silane impregnation agents and weathering topcoats, trial coating with samples, and help writing potential, coulomb, impregnation-depth and pull-off criteria into procurement specifications. Trade terms are EXW/FOB only; no consumer retail is involved. Concrete package proposals and datasheets are confirmed case by case against the project exposure class.
References and data-scope notes
- EN 1504-2: surface protection systems for concrete — criteria for anti-carbonation (Sd,CO2 ≥50 m), adhesion (≥1.0 N/mm²) and vapor permeability (Sd ≤5 m, class I).
- EN 1062 series: test methods and grading for coatings on concrete substrates (vapor, capillary absorption and related classes).
- ASTM C876: half-cell potentials of reinforcing steel in concrete (CSE bands at -200 mV / -350 mV).
- ASTM C1202: electrical indication of chloride permeability (60 V, 6 h, coulomb grading).
- ASTM C1152: acid-soluble chloride in concrete (titration basis of the 0.4% threshold).
- GB/T 50082-2009: Chinese standard for long-term and durability testing of ordinary concrete (RCM rapid migration method).
- GB 50164-2011: Chinese concrete quality control standard (graded chloride limits for the fresh mix).
- JTJ 275-2000: Chinese code for anti-corrosion of marine-port concrete structures (silane dosage and absorption/chloride-uptake acceptance).
- JGJ/T 225-2010: Chinese technical specification for application of rebar corrosion inhibitors (dosage and compatibility testing).
- ISO 12696: cathodic protection of steel in concrete (current density, protection potential and depolarization criteria).
Data-scope note: the D_RCM ranges, inhibitor dosages, penetration depths and corrosion-grade thresholds in this article come from published literature and engineering handbooks as order-of-magnitude references; they are not acceptance values. Acceptance follows the current edition of the standards named in the design documents and contracts.
Last updated: 2026-11-25|Author: Kexin New Materials (Guangdong) Co., Ltd.|B2B technical content for industrial and engineering customers; trade terms EXW/FOB only.