Automotive Craters and Fisheyes: Surface Tension and Silicone

Craters and fisheyes are bowl-shaped pits that form in the wet film, driven by surface-tension differences that spread outward along the edge of a contaminant: a pit ringed by a raised rim with a coating layer still covering the bottom is called a crater, while a pit that penetrates through to expose the substrate is called a fisheye; according to published literature the trigger threshold is only a 1–2 mN/m (dyn/cm) surface-tension difference, and the criterion lies in the Marangoni flow of the wet film and in substrate wettability, not in dry-film hardness or a corrosion-resistance grade. In automotive OEM and refinish coating, the basecoat and clearcoat form the final “mirror layer,” so any low-surface-tension disturbance retracts paint that has already spread out and gets fixed by baking before it can level, which makes craters and fisheyes one of the most frequent appearance defects and among the harder ones to correct after the fact.

A shop that repairs exterior body panels reported that a batch of 2K clearcoat kept coming out of the booth with fisheyes on sunny afternoons, and polishing until the substrate showed meant sanding and respraying. The review pointed to a chain of three causes—the hand-wipe solvent used to clean the body contained silicone, leaving residue in door gaps and folded edges; the air-receiver tank had gone a long time without being drained, so the spray gun carried a trace of oil mist; and, to suppress orange peel, the levelling agent had been temporarily overdosed. With a clearcoat film thickness of only about 40–60 µm, a single low-surface-tension silicone micro-droplet is enough to retract the wet film into a pit, and the high-temperature levelling window after flash and flash-off is too short, so before the pit can flow back it gets frozen by low-temperature cure below 60 ℃. This failure chain shows that controlling craters is not a matter of adding more levelling agent, but of managing three things at once: contamination sources, the wetting criterion, and the re-levelling window.

TL;DR: Quantified criteria you can write straight into a technical agreement

  • The trigger threshold is extremely narrow: per published literature, a region of the wet film only 1–2 mN/m (dyn/cm) lower in surface tension than its surroundings is enough to make a contaminant spread into a pit; if overspray droplets have the same surface tension as the paint, or a higher one, there is no spreading and no pit.
  • Wetting floor: water has a surface tension of 72 mN/m, and typical coating substrates have a surface energy of about 35–45 mN/m (some low-energy substrates < 35 mN/m); to spread and wet, the contact angle θ must be < 90°, and θ>90° beads up immediately (beading).
  • Silicone anti-cratering agents are a quantity that fails once you cross the line: the common optimization window for active content across the full formula is about 0.01%–0.2%; overdosing adds no benefit and instead reduces intercoat adhesion (cross-cut / peel reading).
  • Bake temperature rewrites how silicone behaves: polyether-modified silicone oxidizes at about 140–150℃ (280–300℉) and loses its mobility, and the degradation products act as a barrier layer between two films; polyester / aralkyl-modified types stay stable up to about 220–250℃ (430–480℉).
  • The source is not always in the paint—it can be on the path in: substrate oil, fingerprints, silicone and mold release, compressed-air oil mist, silicone-containing polishing or cleaning aerosols, and incompatible or overdosed defoamers—any one of them can supply a low-surface-tension point.
  • Testing criteria follow standards: wettability per BS EN ISO 19403-5:2024 (pendant drop for σ, goniometer for θ, OWRK / Wu for the components), field dyne values per the 2-second criterion of ASTM D2578 / ISO 8296 / DIN 53364, and contact angle also covered by ASTM D7334.

I. Definition of craters and fisheyes, the morphology scale, and the exposed-substrate boundary

1. Anatomy of a pit: the rim, the center point, and whether it penetrates

On a dry film a crater appears as a bowl-shaped pit about 0.1–2 mm across, with a raised ring around the edge that closed back after being pulled open (the crater rim), and often a residual contaminant particle or incompatible droplet at the center. The first cut in judging is whether it reaches the bottom: as long as a continuous coating layer still covers the substrate at the pit floor, it is called a crater in engineering; when the pit penetrates the whole wet film and exposes the primer or substrate beneath, it is called a fisheye. Fisheyes are more serious than craters because they break both appearance and the barrier (corrosion, stone-chip, and insulation protection), and rework usually means sanding back to intact area and recoating. This is different from the edge problem handled in our automotive refinish masking: tape peel-force window, temperature-ageing resistance, and edge bleed control article—masking deals with interfaces and paint lines, while craters deal with wetting collapse across the whole film surface.

2. Do not mistake a crater for a pinhole or orange peel

The three look alike but have different causes; judge the direction wrongly and the rework is wasted. A pinhole is an open hole left by air trapped in the wet film or by escaping solvent, following the solvent-retention and flash-off logic; it relates to the surface condition discussed in our laser cleaning as pre-coating surface preparation: energy density, roughness, and adhesion acceptance criteria article, but it is not a tension collapse. Orange peel is a rippled surface from insufficient levelling, judged by distinctness-of-image DOI—see our control of coating orange peel and its relation to DOI article. The signature of a crater is an isolated round pit plus a rim plus, usually, a low-tension center point, whereas orange peel is continuous undulation and a pinhole is a point hole with no rim.

II. Marangoni flow: how a 1–2 mN/m tension difference tears open a pit

The kinetics of pit formation is Marangoni flow—liquid motion driven by a surface-tension gradient. A liquid always tends to shrink its surface area to as small as possible; when a local region of the wet film has lower surface tension than its surroundings, the higher-tension paint nearby is pulled away from this low-tension point, dragging paint—pit and rim together—outward and exposing a depression. The triggering difference given in published literature is extremely small: a surface-tension difference of 1–2 mN/m (dyn/cm) is enough to make a low-tension droplet spread and form a crater; conversely, if an overspray droplet has the same surface tension as the paint, or a higher one, no spreading occurs and thus no pit. This also explains why, within the same panel and the same oven, some parts pit and others do not—it comes down to that 1–2 mN/m.

Illustration of edge pull-in, fat edge, and thick edge defects in automotive spraying, used to understand how surface-tension-driven liquid migration (cratering and edge pull-in share a cause) is amplified at geometric edges

1. Where contamination sources come from: substrate, air supply, and the formula itself

Low-surface-tension points enter through three gateways. The first is brought in by the substrate: assembly oils, mold-release residue, sweat fingerprints, a previous polishing or silicone cleaning aerosol (containing cyclosiloxanes), and silicone sealant migrating from folded edges or weld seams. The second is brought in by the air supply and the process: an air receiver not regularly drained of water and oil, the spray gun carrying a trace of oil mist, or overspray of a silicone-containing aerosol from an adjacent station landing on a wet film that is still fluid. The third is brought in by the formula: a defoamer is itself a partially incompatible system, and too high a dosage or poor dispersion becomes a low-tension point inside the film; switching a resin lot or blending auxiliaries of different polarity can also pull the tension down somewhere. The effect of pretreatment degreasing and interface state on wetting shares a root with our automotive body coating pretreatment: phosphate, thin-film zirconium, and phosphorus-free route selection article—only that one addresses adhesion and corrosion resistance, while here we focus on whether it wets enough and whether it will be broken by a low-tension point.

2. Low-energy substrates are an amplifier: basecoat aluminum-flake orientation also depends on wetting

Low-surface-energy substrates (such as untreated PP/PE plastic parts and some clearcoat recoat surfaces) are already near the 35 mN/m lower limit or below it; for paint to spread on them the wet-film surface tension must be reduced below the substrate critical surface tension, and once a silicone micro-droplet is added on top, the probability of a pit rises sharply. The orientation of aluminum flakes and pearlescent pigments in a metallic basecoat (the flop, color travel, or floating) likewise depends on a uniform, fully wetted wet-film base, and orientation defects and craters often share a cause—both point to whether the wet film was spread out completely, which can be understood together with our basecoat metallic aluminum-flake orientation and flop control article.

III. Surface tension, critical surface tension, and contact angle: writing wetting into measurable numbers

To turn can-it-wet-or-not into a number, use the three-piece set: liquid surface tension σlv, solid (critical) surface tension σc, and apparent contact angle θ. The two anchors given by published reviews are that water has a surface tension of 72 mN/m and the typical surface-energy level of coating substrates is about 35–45 mN/m, with some low-energy substrates below 35 mN/m. The criterion is the Young equation and the spreading coefficient: when θ < 90° the droplet tends to spread and wet, and when θ > 90° it beads up directly; to make a waterborne system wet a 35–45 mN/m substrate, a wetting agent must lower the paint surface tension below the substrate critical surface tension—which is exactly why 72 mN/m water is innately non-wetting and has to be adjusted with surfactants.

Table 1 Definitions of the three wetting quantities, typical values, and the is-it-enough-to-spread criterion (values follow published standard methods and literature)
Physical quantitySymbol / unitTypical value or referenceCriterion / meaning
Liquid (paint) surface tensionσlv / mN/m (= dyn/cm)Water 72; a waterborne formula must be lowered below the substrate critical value; example formula σld≈38Determines whether spontaneous spreading occurs; too high leads to shrinkage into a pit
Solid (critical) surface tensionσc / mN/m (= mJ/m²)Typical coating substrate 35–45; low-energy substrate < 35 (untreated PP/PE lower still)σlv must be below σc in order to wet
Apparent contact angleθ / ° (degrees)Example: against PTFE (σsd=18.5 mJ/m²) θ=72°θ<90° wetting; θ>90° beading, no wetting
Polar / dispersion componentsσsd, σsp / mJ/m²OWRK or Wu equation back-calculates them from multi-liquid θLow σsp surfaces are hard to wet with high-polarity paint
Dyne value (field quick test)dyn/cm (= mN/m)Dyne liquids / pens graded 38, 40, and so on; a 2-second no-retraction is judged wettedField check of whether the substrate reaches the target σc

IV. Differentiation from adjacent defects: orange peel, pinholes, Bénard cells, and edge pull-in

The first step of appearance rework is to pick the crater out of the other pits. Bénard cells are honeycomb patterns caused by convective turbulence in the wet film during drying, related to pigment turbulence within the film; the cause is rheology and a solvent-evaporation gradient rather than an external low-tension point. Edge pull-in, or crawling, is the paint retracting wholesale from an edge or low-tension region and exposing an edge band. Telegraphing and base mottling (brassing) print different surface-tension regions of the substrate up onto the topcoat. Their treatment is entirely different from that of a true silicone-contamination crater: the contamination type needs source-cutting plus a wetting agent, the rheology type needs formula and flash-off window control, and the edge type needs a film-thickness and viscosity balance.

Table 2 Distinguishing features and primary causes of craters versus adjacent appearance defects (mechanism categories follow published literature)
DefectMorphological featurePrimary causePrimary treatment direction
CraterIsolated bowl pit with a rim, often with foreign matter at the centerLocal low-surface-tension point (contamination or additive)Cut the source, lower σlv, and widen the levelling window
FisheyePit that penetrates to expose the substrateSame as a crater but deeper, with the barrier brokenSand to intact area and recoat; remove the contamination source first
PinholeFine open hole with no rimTrapped air or escaping solventDefoaming plus the flash-off and film-thickness window
Bénard cellsHoneycomb convection patternFilm turbulence and evaporation gradient during dryingRheology and solvent balance, reducing convection
Crawling (edge pull-in)Edge band retracts wholesale, exposing the bottomEdge σ gradient plus viscosity imbalanceFilm thickness and viscosity, edge wetting
Orange peelContinuous rippled undulationInsufficient levelling (not collapse)Atomization, flash-off, and levelling (DOI criterion)

V. Formula and process windows: levelling agent, anti-cratering dosage, and bake boundaries

The formula-side lever is a weighing of two harms: you must lower the paint surface tension in order to wet and to shield contamination points, yet not sacrifice intercoat adhesion and recoatability. The principle given by published supplier technical literature is that polyacrylate levelling agents mainly improve levelling and have a limited effect on surface tension, so they are not used on their own as anti-cratering agents; strong tension reduction and anti-cratering rely on (modified) polysiloxanes. Silicone anti-cratering agents have a clear dosage window that fails once you cross it: on active content across the full formula, published examples give three tiers, 0.01% / 0.05% / 0.2%; below the lower limit you cannot shield contamination points, and above the upper limit the molecules linger at the interface of the two films as a barrier layer, and cross-cut and peel adhesion clearly worsens. For a specific anti-fisheye or anti-silicone additive, the supplier TDS operating guidance is blunter: one product is added at 1 measure part per liter (or quart), mixed, then matured for about 10 minutes, never overdosed, and not used in primer systems; another solvent-borne product is labeled 1 oz/gal, upper limit 3 oz/gal, and its VOC can reach about the 751 g/L level—adding it also raises VOC, so it has to be weighed together with environmental targets. This is one and the same with the flash point, cure, and application mutual constraint discussed in our automotive refinish 2K clearcoat: low-temperature cure, flash point, and application essentials article.

Close-up of coating particles, paint filtration and oil-water separation, and a standardized enclosed spray booth, used to illustrate how air-supply oil mist and overspray contamination supply low-surface-tension points to the wet film

1. Bake temperature rewrites the silicone fate: 140–150℃ oxidation and 220–250℃ tolerance

Whether silicone can finish its job and leave (migrating to the next surface and not remaining at the interface) depends on bake temperature. Published literature notes that polyether-modified silicone oxidizes above its tolerance temperature—oxidation begins at about 140–150℃ (280–300℉), the reactive groups lock it into the coating so it loses mobility, and the degradation products left between the two films act as a barrier layer that weakens intercoat adhesion; for high-temperature baking you should switch to polyester / aralkyl-modified silicone, stable up to about 220–250℃ (430–480℉). The engineering meaning is that the right dosage and selection for the same anti-cratering agent in a 60 ℃ low-temperature refinish and a 140 ℃ OEM bake may be completely different, and the dosage window must be set together with the bake curve.

2. The re-levelling window: is there enough time to flow the pit back

After a pit forms, as long as the wet film stays fluid for some time and the surface-tension gradient still has time to pull the edge flat, the pit can self-heal; once solvent release drives a sudden viscosity rise or cure begins, the pit is frozen. So controlling craters is not only about not contaminating—it also includes designing the flash-off and levelling window to be wide enough to flow micro-pits back, which is tied to atomization, film thickness, the number of spray passes, room temperature, and forced-flash temperature and humidity, and which shares the same time-and-viscosity curve as the orange-peel levelling criterion in the previous section.

Table 3 Anti-cratering windows and criteria on the formula and process side (dosages and temperatures follow published suppliers and literature)
LeverWindow / valueConsequence of crossing the lineReading method
Silicone anti-cratering dosageActive content about 0.01%–0.2% (across the full formula)Too low gives no shielding; too high damages intercoat adhesionStepped test panels plus cross-cut / peel
Levelling-agent type divisionPolyacrylate for levelling; polysiloxane for tension reduction and anti-crateringWrong type: craters persist or levelling is insufficientCombination screening (silicone / acrylate)
Anti-fisheye additive handling1 measure part per liter (or 1 oz/gal, upper limit 3 oz/gal), matured about 10 minutesOverdose gives a barrier layer and raises VOC (up to about 751 g/L)Shipped TDS plus VOC accounting
Bake temperature and silicone selectionPolyether-modified oxidizes at 140–150℃; polyester / aralkyl-modified tolerates 220–250℃High temperature locks the silicone and lowers intercoat adhesionSet the dosage together with the bake curve
Re-levelling windowFlash-off, viscosity, and cure time must be enough to flow micro-pits backA too-short window freezes the pits and rework exposes the substrateBetween-pass interval plus forced-flash temperature and humidity
Air-supply cleanlinessDrain the receiver regularly; eliminate oil mist and silicone-containing oversprayLow-tension points keep entering the wet filmCompressor-station water and oil monitoring

VI. Testing and acceptance: dyne value, contact angle, and ISO 19403 / ASTM D2578 / D7334

To accept by numbers rather than by eye, you have to ground substrate wettability and the paint σ and θ in standard methods. Systematic measurement of wettability follows BS EN ISO 19403-5:2024: first measure the liquid surface tension by the pendant-drop method (corresponding to ISO 19403-3), then measure the contact angle with non-polar reference solids (PTFE / paraffin) and an optical goniometer, then use the OWRK or Wu equation to compute the polar and dispersion components of the surface energy; the 2024 edition tightens the contact-angle uncertainty to static ±1° and dynamic ±3° (±2° in the 2020 edition), specifies the environment 23±2℃ / 50±5%RH, a reference solid of Ra < 0.3 µm, and ≥ 10 measurements per point. Field quick testing uses the dyne method: ASTM D2578 (PE/PP film), ISO 8296 (plastic film / sheet), and DIN 53364 all use a series of dyne liquids or pens of known tension, judging that the dyne value has been reached when the liquid film stays continuous without retracting within about 2 seconds. The contact-angle and advancing-angle method is covered separately by ASTM D7334. What these methods give is the criterion of whether the substrate is wettable enough and whether the paint surface tension has already dropped below the threshold; crater acceptance should also add defect counting (pits per ㎡, pit diameter, and whether the substrate is exposed) together with rework accessibility.

VII. Key data quick reference (with units)

  • Crater trigger tension difference: 1–2 mN/m (dyn/cm); no pit forms when tensions are equal or the overspray droplet has a higher tension (published-literature reference).
  • Water surface tension 72 mN/m; typical coating substrate surface energy 35–45 mN/m, with some low-energy substrates < 35 mN/m.
  • Wetting criterion: θ < 90° spreads and θ > 90° beads; example formula σld≈38 mN/m against PTFE (σsd=18.5 mJ/m²) θ=72°.
  • Silicone anti-cratering active-content window: 0.01% / 0.05% / 0.2% (across the full formula); overdosing damages intercoat adhesion.
  • Bake boundary: polyether-modified silicone oxidizes and deactivates at about 140–150℃ (280–300℉); polyester / aralkyl-modified tolerates about 220–250℃ (430–480℉).
  • Crater and fisheye pit diameter is commonly 0.1–2 mm; an automotive topcoat or clearcoat dry film is about 40–60 µm, so pits easily penetrate to expose the substrate.
  • Testing reference: ISO 19403-5:2024 static ±1° and dynamic ±3°, environment 23±2℃/50±5%RH, Ra < 0.3 µm, ≥10 per point; a dyne-liquid 2-second no-retraction criterion; anti-fisheye additive VOC can reach about 751 g/L.

VIII. Frequently asked questions (FAQ)

Q1: Are a crater and a fisheye two defects or one?

Same mechanism, two depths. Both form when a local low-surface-tension point in the wet film pulls the paint away through Marangoni flow, and both look like round pits with a rim. The difference is penetration: a pit floor still covered by a continuous coating layer over the substrate is a crater, while a pit that penetrates the whole layer and exposes the primer or substrate is a fisheye. Because an automotive clearcoat or topcoat film is only about 40–60 µm thick, a pit 0.5–2 mm across easily penetrates, so in the field the two are often used interchangeably—but acceptance should separate them: a fisheye breaks appearance plus the barrier (corrosion protection, insulation, and stone-chip resistance), while a crater mainly breaks appearance, so the treatment intensity differs.

Q2: Why does adding more levelling agent often make things worse?

Because a levelling agent and an anti-cratering agent are not the same thing, and both have a window that fails once you cross it. Published supplier guidance notes that polyacrylates mainly improve levelling with a limited effect on surface tension, so expecting them to hold down a silicone-contamination crater is often ineffective; real strong tension reduction relies on modified polysiloxanes. And the suitable window for silicone active content is commonly between 0.01%–0.2% (across the full formula)—below the lower limit you cannot shield contamination points, and above the upper limit silicone molecules linger at the interface of the two films as a barrier layer, cross-cut and peel adhesion clearly worsens, and recoating and intercoat delamination may follow. So the correct order is to cut the contamination source first, then set the dosage by a stepped test, rather than simply adding more levelling agent.

Q3: Why, in the same oven, do some panels pit and some not?

It comes down to that 1–2 mN/m. The trigger threshold for pit formation is extremely narrow: as long as a local region of the wet film is only about 1–2 mN/m lower than its surroundings, it is enough to let a contaminant spread into a pit; conversely, if the tensions are equal or the overspray droplet has a higher tension, no pit forms. And whether that 1–2 mN/m low-tension point exists is highly random—it depends on whether this panel was wiped clean, whether a silicone aerosol landed on it, whether the air supply carried oil mist at that pass of the gun, and whether this batch of re-blended additives was compatible. So the problem is rarely that the paint is bad, and more often a contamination event on this panel, at this pass, at this moment. Cutting the source (clean wiping, draining oil and water from the air supply, and isolating silicone-containing stations) is more fundamental than adjusting the paint.

Q4: Can a low-temperature refinish cure and a high-temperature OEM bake share one anti-cratering agent?

Not necessarily; the key is that bake temperature rewrites the silicone fate. Polyether-modified silicone begins to oxidize at about 140–150℃ and loses its mobility, and degradation products left between the layers weaken adhesion; so a polyether-modified silicone that works well in a 60 ℃-grade low-temperature refinish can become an adhesion risk at a 140 ℃ OEM bake. For high-temperature systems choose a polyester / aralkyl-modified silicone (published literature gives stability up to about 220–250℃) and set the suitable dosage together with the bake curve. Directly reusing the same anti-cratering agent across low-temperature refinish and high-temperature OEM is risky precisely along that oxidation-temperature line.

Q5: How do you judge on the spot in the shop whether a substrate can wet, rather than waiting for a pit?

Use the dyne method as a pre-check. Following wetting-tension methods such as ASTM D2578 / ISO 8296 / DIN 53364, draw a line on the substrate with a series of dyne liquids or pens of known surface tension (graded 38, 40, and so on); if the liquid film stays continuous within about 2 seconds without retracting into beads, the substrate surface tension is taken to reach or exceed that value. Align the target paint σlv with that dyne value (the paint tension must be below the substrate critical tension, and the contact angle θ<90°), and you can predict before coating whether it will hold the wetting. For stricter polar and dispersion surface-energy components, follow BS EN ISO 19403-5:2024 with a goniometer plus OWRK / Wu back-calculation, which suits incoming-material verification and dispute arbitration.

Q6: Once a fisheye has appeared, can it be polished out or must it be resprayed?

It depends on whether the substrate is exposed and on the count. Shallow craters that do not penetrate and are few in number can be treated locally while widening the levelling window, but the safer practice is to first identify and cut the contamination source (otherwise recoating will grow new pits), then sand to intact area and recoat. A fisheye that already exposes the substrate has broken the barrier, and polishing cannot recover film thickness or the insulation and corrosion-protection function, so you must sand out the edges of the penetrated area and recoat the matching coat system—this is exactly where it differs from orange peel, which can be polished while craters are hard to save. If, before rework, you do not resolve the three source types of air-supply oil mist, silicone-containing hand-wipe solvent, and mold-release residue, respraying just fixes the pits once more.

Q7: Are silicone-containing polishes and cleaners a common nemesis in automotive coating?

In actual complaints, silicone is almost always the prime suspect. Cyclosiloxanes and silicone come from polishing wax, silicone-containing cleaners and aerosols, and migration from some sealants; they have extremely low surface tension, a few micrograms landing on the wet film can create a low-tension point that triggers Marangoni pit formation, and silicone migrates back and forth across the body and the stations with each wipe, so its contamination range far exceeds a point. The countermeasure is zoning: use silicone-free degreasing and cleaning agents for pre-coating pretreatment and wipe-down, physically isolate silicone-containing stations (polishing, sealing, and repair) from the spray area with separate exhaust, and add oil and water removal and filtration to the air supply. This points the same way as the interface cleanliness emphasized in our body pretreatment article, only here the focus is not to bring a 1–2 mN/m low-tension contaminant into the topcoat.

Q8: Can we claim that there will be no craters at all and never any fisheye?

You cannot write that—it both violates compliance rules and cannot be verified. The compliant wording gives criteria and conditions: for example, measured per BS EN ISO 19403-5:2024 at 23±2℃/50±5%RH, this paint has σlv=X mN/m and θ=X° (<90°) against the target substrate; a dyne pre-check of the substrate of ≥Y dyn/cm; a silicone anti-cratering active-content dosage of Z% (set by stepped test); within the window of a W℃ bake and a T-minute between-pass flash, the defect count is N pits per ㎡, pit diameter ≤D mm, with no substrate exposed. It should also state that these are determinations made under published standard methods and supplier or literature references, with the shipped report, the contract appendix, and the official standard text being final. Blanket statements that there will not be a single defect constitute unverifiable claims and do not meet B2B technical-wording standards.

IX. References and notes on sources

Notes on sources: First, the 1–2 mN/m trigger threshold, the silicone active-content 0.01%–0.2% dosage window, the 140–150℃/220–250℃ oxidation tolerance, and values such as 72/35–45 mN/m and θ=72° in this article are reference wording from published standard methods, textbooks, and supplier technical tables, used to explain the mechanism and the order of magnitude, not guaranteed measured values from our plant or a specific batch. Second, the addition ratios, maturation time, and VOC values of anti-fisheye and anti-cratering additives come from the corresponding supplier TDS; actual use follows the shipped TDS and formula-compatibility tests, and a type or lot change requires repeating the stepped test. Third, dyne values, contact angles, and surface-energy components depend heavily on cleanliness and environment (23±2℃/50±5%RH) and cannot be directly compared across lots or across instruments; the criterion follows the relative trend from the same instrument under the same conditions. Fourth, the on-site cause combinations for craters and fisheyes vary widely; this article is B2B technical reference material and does not constitute a conformity judgment of any specific panel, batch, or test result, nor does it involve the issuance or validity of any certification.

Kexin New Materials (Guangdong) Co., Ltd. supplies functional coatings and supporting solutions as B2B technical reference material for automotive OEM and refinish coating, pretreatment, and coating-process departments; trade terms are agreed as EXW or FOB; the performance indicators, test methods, and application boundaries of a specific batch follow the contract appendix, the technical data sheet, and an acceptance plan confirmed by both parties.

Last updated: 2026-11-16
Kexin New Materials (Guangdong) Co., Ltd.
This article is B2B technical material for automotive OEM and refinish coating departments; trade terms are agreed only as EXW or FOB; the performance indicators, test methods, and application boundaries of a specific batch follow the contract appendix, the technical data sheet, and an acceptance plan confirmed by both parties.

Tags: #Automotive coatings #Automotive Coatings #Coatings technology literature