Zn-Al-Mg coated steel is one coating system inside the continuous hot-dip coated steel sheet family: a ternary zinc-aluminum-magnesium alloy coating is applied to the strip surface. EN 10346:2015 writes this class of hot-dip coating designation as ZM and specifies that aluminum plus magnesium in the coating bath totals 1.5%–8%, that magnesium is not less than 0.2%, and that the balance is zinc. The current Chinese product standard GB/T 2518-2019 for continuous hot-dip zinc and zinc-alloy coated steel sheet and strip covers four coating types — pure zinc (Z), zinc-iron alloy (ZF), zinc-aluminum alloy (ZA) and aluminum-zinc alloy (AZ) — over a thickness range of 0.20 mm–6.0 mm, so Zn-Al-Mg strip is in practice ordered against a mill's works specification, against the ZM system of EN 10346, or against the YZAM Zn-Al-Mg designation given in GB/T 31447-2015 for pre-galvanized highway guardrails. What follows is not about the corrosion resistance of an unbroken surface but about whether the bare steel exposed by shearing, punching and forming can be protected, and whether an extra layer of paint is needed.
A Zn-Al-Mg solar mounting rail is flame-cut by the installation crew on site, while the other end has had rows of mounting holes punched in the factory on a precision press. Look back after three to five years of service and the two ends have aged completely differently: the coating around the punched holes is still bright, whereas the flame-cut end has gone red from the face inward and is rusting through the hollow section from the inside out, with the outside coating apparently intact and rust flakes packed inside the cavity. The project team's first reaction is usually that the wrong material was bought, and the laboratory report on a sample section sent in for testing shows the coating composition meets specification. The real problem is treating cut-edge self-healing as an unconditional promise. The material source of self-healing is the surrounding coating, and how far it reaches is set jointly by the supply area of coating, the sheet thickness, the exposed area, ambient humidity and chloride deposition; the heat-affected layer and dross on a site-cut face then degrade the conditions for a protective film to form even further.
TL;DR: seven points to hold on to
- The criterion is an area ratio, not a self-healing radius: the published ring test (Corrosion and Protection, 2024, 45(12)) laser-cut annular specimens and varied the ratio of cut-edge area to coating area; resistance to red rust at the cut was good below a ratio of 0.5, and the red-rust area grew as the ratio increased.
- Converted into part geometry: for a ring the ratio is close to the sheet thickness t divided by twice the ring width, and for a square panel it equals 2t/L; it lands on 0.5 when the side is 4 times the thickness (or when the ring width equals the thickness), which makes thick plate, small parts and densely spaced large holes high-risk cuts.
- Order-of-magnitude years come from a linear estimate on the ISO 9223 first-year corrosion rate for zinc: a 25 µm single-side coating lasts roughly 12–36 years in C3 (0.7–2.1 µm/a), 6–12 years in C4 (2.1–4.2 µm/a) and 3–6 years in C5 (4.2–8.4 µm/a) — pre-selection only, and ISO 9224 notes that long-term rates are usually lower.
- Magnesium conditions the corrosion products instead of forming a film itself: Mg²⁺ precipitates as Mg(OH)2 and buffers pH, raising the share of zinc hydroxychloride Zn5(OH)8Cl2 in the cut-edge products (Corrosion Science 2019, 160: 108170), yet XRD after 24 h of salt spray showed no diffraction peak of any magnesium-bearing product.
- Judge the paint scheme at the interface first: an alkaline pretreatment strips the initial oxides and dissolves Al selectively (DOI 10.1016/j.surfcoat.2020.126236), and residual passivation or anti-fingerprint films plus the zinc soap weak boundary layer are the two main adhesion risks (Prog. Org. Coat. 2015, 83: 26).
- White rust is a storage and handling condition: zinc surfaces react faster at relative humidity near 60% or 85%–95%, water-film pH below 6 and about 70 ℃; the surface code sets the window, and the reproduced Q/BQB 420—2023 requirement for 5% white-rust coverage in salt spray is 96 h for SL2 against 48 h for C and IC.
- Years must not be written into an acceptance clause: ISO 12944-1:2017 grades durability as L (up to 7 years), M (7–15 years), H (15–25 years) and VH (more than 25 years) and states that durability is not a warranty period, so externally one specifies only the corrosivity category, the nominal dry film thickness and the three re-inspection items — adhesion, salt spray and soluble salt.
The coating system first: ZM bath-composition limits and solidified microstructure
Draw the boundary of the system first. Under the bath definition for ZM in EN 10346:2015, the combined aluminum-plus-magnesium ceiling is 8%, and the low-aluminum low-magnesium grades common in China (Al 1%–3%, Mg 1%–1.5%, Si about 0.1%) fall inside that window: the knife coater can be purged with ordinary air and the alloy melts at about 380 ℃. The Japanese route, Zn-11%Al-3%Mg-0.2%Si, totals about 14% aluminum plus magnesium and therefore crosses the ZM bath-composition boundary on a literal reading; published material treats it as a separate high-aluminum high-magnesium route and requires nitrogen purging for thickness control. The practical conclusion: do not equate performance on the strength of the words 'zinc-aluminum-magnesium' alone — read the bath composition, the coating designation and the per-side coating thickness stated on the mill certificate. Watch the version timeline as well. EN 10346:2015 states its applicable thickness as 0.20 mm ≤ t < 3.0 mm, while the DIN draft dated 2025-06 and the published BS EN 10346:2026 (issued 2026-10-28) extend the range to 0.20 mm–6.5 mm and add designation A for pure aluminum coating. Above 3 mm plate, the standard version quoted in the contract changes the acceptance basis directly.
1.1 Single phase, binary eutectic, ternary eutectic: microstructure sets the corrosion path
The study on cut edges of zinc-alloy coating systems published in the Journal of the Chinese Society for Corrosion and Protection, 2026, 46(3), supplies a microstructure map that can be used directly in failure analysis: a pure zinc coating is an η-Zn free layer over the δ-FeZn10 and ζ-FeZn13 intermetallic layers; a Zn-Mg coating is dominated by a lamellar η-Zn/MgZn2 binary eutectic with no coarse single phase; a Zn-Al coating is an η-Zn/α-Al binary eutectic plus coarse η-Zn single phase, with an Fe2Al5Znx layer at the interface; and a Zn-Al-Mg coating contains all three at once — an η-Zn single phase that is smaller and less abundant, the η-Zn/MgZn2 binary eutectic and the η-Zn/α-Al/MgZn2 ternary eutectic — with the ternary eutectic finer than the binary one. The intermetallics magnesium forms with zinc are MgZn2 and Mg2Zn11, and published work notes that titanium and boron micro-alloying suppress the formation of Mg2Zn11. Below 13% aluminum by mass no independent aluminum-bearing phase forms; aluminum exists inside the eutectic. Why does microstructure matter? Because corrosion initiates at the eutectic regions: the zinc-rich phase is where cathodic oxygen reduction concentrates, the anodic reaction runs in the eutectic, and the direction and strength of the micro-galvanic couple are set by how those phases are distributed in space.
What actually happens at the cut edge: anodic-cathodic loop and product distribution
The cut edge is a microscopic cell in which the coating is the anode and the exposed steel substrate is the cathode. In the 2026 in-situ study cited above, immersion in 5% NaCl solution deposits corrosion products first on the steel side adjacent to the coating and only then spreads them toward the coating surface; on the steel side away from the coating almost nothing forms because the diffusion distance for Zn²⁺ is too long. After 6 h of immersion the height difference between steel substrate and coating at the cut edge was 9.7, 6.2, 5.7 and 5.1 µm for pure Zn, Zn-Mg, Zn-Al and Zn-Al-Mg respectively. On the coating side the products are dominated by Zn5(OH)8Cl2; on the steel side they are a mixture of Zn5(OH)8Cl2 and Zn5(OH)6(CO3)2·H2O, and aluminum-bearing systems add the layered double hydroxide Zn6Al2(OH)16CO3·4H2O. A pure zinc coating generates a large volume of surface product, but it is loose, full of pores and cracks, so its protective value is limited — which is why pure zinc cut edges corrode badly under the same salt-spray conditions.
| Coating system | Solidified microstructure | Mean cut-edge mass-loss rate after 24 h salt spray g/(m·h) | Main cut-edge corrosion products | Height difference after 6 h immersion µm |
|---|---|---|---|---|
| Pure Zn | η-Zn free layer plus δ-FeZn10 and ζ-FeZn13 intermetallic layers | 0.0104 | Mostly Zn5(OH)8Cl2, loose and porous structure | 9.7 |
| Zn-3Mg | Lamellar η-Zn/MgZn2 binary eutectic, no coarse single phase | 0.00988 | Zn5(OH)8Cl2 | 6.2 |
| Zn-5Al | η-Zn/α-Al binary eutectic plus coarse η-Zn, Fe2Al5Znx at the interface | 0.00573 | Zn5(OH)8Cl2, Zn5(OH)6(CO3)2·H2O, Zn6Al2(OH)16CO3·4H2O | 5.7 |
| Zn-4Al-3Mg | Less η-Zn single phase, with binary and η-Zn/α-Al/MgZn2 ternary eutectic | 0.00521 | As above, with a flat, dense, crack-free product layer | 5.1 |
2.1 What magnesium does, and what it does not do
Magnesium's role is cross-checked by three independent sources. Suzuki et al. ran wet-dry cycling on Zn-11%Al-3%Mg-0.2%Si (ISIJ International 2020, 60: 2038): red rust appeared on the cut edge of the pure zinc sheet and not on the Zn-Al-Mg coating; zinc-bearing white rust covered the center of the cut edge over a larger area; and polarization tests showed that the white rust suppresses both the anodic and the cathodic current density on the steel substrate, leaving a smaller galvanic current between coating and substrate. Lee et al. supply the chemical explanation (Corrosion Science 2019, 160: 108170): Mg²⁺ precipitates as Mg(OH)2 and buffers pH, which raises the share of Zn5(OH)8Cl2 in the cut-edge product layer. Tokuda et al. (Corrosion Science 2023, 225: 111605) place the starting point in the preferential dissolution of the magnesium-bearing phase. The same in-situ dataset also shows the other side of the picture: after 24 h of salt spray no diffraction peak of any magnesium-bearing corrosion product was observed in the XRD patterns of the four coatings, and the dense, low-conductivity, shielding phases are still Zn5(OH)8Cl2 and the aluminum-bearing Zn6Al2(OH)16CO3·4H2O. Magnesium therefore conditions the corrosion products instead of growing a film of its own.
The self-healing boundary: area ratio is more reliable than a self-healing radius
Claims circulating on trading platforms — a self-healing radius of 3 mm, or a 1 mm cut repaired within 72 hours — come with no published specimen geometry, salt-spray condition or acceptance scale, so they cannot be used as design inputs. The auditable criterion is an area ratio. The Shougang Research Institute of Technology team laser-cut Zn-Al-Mg plate of several thicknesses into annular specimens of varying inner and outer diameter and systematically varied the ratio of cut-edge area to coating area (Corrosion and Protection, 2024, 45(12)): under neutral salt spray the red-rust area at the cut grew steadily as the ratio increased, and cut-edge resistance to red rust was good below a ratio of 0.5. The value of this criterion is that one number contains sheet thickness, part size and processing method together, whereas a self-healing radius describes only one of the three.
3.1 Converting the area ratio into part geometry
Derived from the annulus geometry: the cut-edge area is approximately 2π(r_inner + r_outer)·t and the two-side coating area 4π(r_outer² − r_inner²), so the ratio is close to t divided by twice the ring width, and it equals 0.5 when t equals the ring width. For a square panel of side L and thickness t the cut is 4L·t and the coating 2L², so the ratio equals 2t/L and lands on 0.5 when the side is 4 times the sheet thickness. Some realistic orders of magnitude: a 1.5 mm plate with 10 mm of effective supply band around a hole gives 0.075, comfortably on the safe side; shrink the supply band to 1.5 mm and the ratio is 0.5, right at the boundary; a 2.0 mm plate cut into 8.0 mm squares gives exactly 0.5; a 4.0 mm thick block with a 30 mm side gives 0.27. Whether a cut edge is protected is therefore first a geometric question and only then an environmental-chemistry question — thick plate, small parts, densely spaced large holes and site thermal cutting either thin the supply area or inflate the exposed area, and self-healing stops being a possibility. (These conversions are derived here from specimen geometry to establish an order-of-magnitude judgment; they are not clauses of any standard.)

Coating designations and corrosivity categories: the multiples are not linear
A coating designation states the total coating mass on both sides in g/m², so convert to per-side thickness before comparing anything. For pure zinc, at a coating density of about 7.1 g/cm³, Z275 works out to roughly 20 µm per side; Zn-Al-Mg is slightly less dense, and published data put ZM120 / ZM250 / ZM310 / ZM430 at roughly 10 / 20 / 25 / 35 µm per side. The same g/m² figure means a different thickness in the two coating families, so cross-system price comparison and acceptance should be written in per-side thickness, or as designation plus mill certificate, otherwise the order is placed on coating mass and the film actually delivered is thinner. As for 'N times the corrosion resistance of pure zinc', published supplier literature spans 3–5 times, 5–10 times and 10–20 times, and the spread comes from the alloy route (low-aluminum low-magnesium versus high-aluminum high-magnesium), the specimen condition (flat panel, cut edge, bent, strained) and the test method. GB/T 10125-2021 and ISO 9227:2017 themselves state that a salt-spray test is not applicable to ranking the corrosion resistance of different materials, and still less to predicting service life.
| Corrosivity category | Typical environment (informative) | First-year thickness loss for zinc µm/a | Linear consumption of 25 µm coating | Specification tier |
|---|---|---|---|---|
| C1 very low | Heated interiors with clean air | 0.1 and below | More than 250 years | Coating alone in most cases |
| C2 low | Unheated stores, dry inland climates | 0.1–0.7 | About 36–250 years | Coating alone |
| C3 medium | Urban and light industrial atmosphere, low-salinity coastal | 0.7–2.1 | About 12–36 years | Coating alone or decorative painting |
| C4 high | Industrial and coastal atmospheres of moderate salinity | 2.1–4.2 | About 6–12 years | A paint scheme should be assessed |
| C5 very high | High-humidity, high-salinity industrial and near-shore | 4.2–8.4 | About 3–6 years | Coating system plus cut-edge touch-up |
| CX extreme | Offshore, tidal zone and extreme salt spray | 8.4–25 | About 1–3 years | Designed separately per ISO 12944-9:2018 |
A linear estimate built on the first-year corrosion rate for zinc given in ISO 9223 turns a designation into an order-of-magnitude figure in years, usable for pre-selection and not as a commitment. ISO 9224 notes that long-term rates are usually lower than the first-year rate, so the table below errs conservative; real behavior also depends on orientation, water retention and time of wetness, pollution and wash-off frequency. ISO 12944-2:2017 likewise stresses that the classification rests on the first-year mass or thickness loss of reference specimens, prefers measured data from site-exposed specimens, and treats the typical environment examples as informative — inside one plant, sheltered steel, steel that condenses continuously and steel that collects chloride deposition can fall into different corrosivity categories.

Storage, handling and fabrication: white rust, scratches and the chain that leads to painting
White rust is a storage and handling problem, not a metallurgical failure of the coating. The causal chain is clear: coiling or packing at too high a temperature, condensation inside the package, water ingress left unaddressed, poor ventilation of the stack, and sheets piled with condensate on the surface. Published data give the sensitive range as relative humidity around 60% and 85%–95%, water-film pH below 6, and faster zinc-surface reaction at about 70 ℃ — in other words a warehouse that is neither very dry nor very wet is riskier than a dry one. For the coating work that follows, white rust matters because it is a loose, water-bearing interface with unstable conductivity: treat it as something a rinse fixes and spray straight over it, and pull-off adhesion falls below the acceptance line after damp-heat cycling.
6.1 Surface post-treatment sets the storage window and the painting difficulty
The mill's surface post-treatment code sets both the storage window and the difficulty of painting. Common codes are chromate passivation (C), passivation plus oiling (CO), chrome-free passivation (CN or C5), anti-fingerprint coating (AF / N5), self-lubricating coating (SL / SL2), inorganic passivation (IC / ICO), inorganic self-lubricating (SW), oiled (O) and untreated (U). Taking the white-rust salt-spray acceptance times reproduced from the Baoshan Iron & Steel Co., Ltd. works standard Q/BQB 420—2023: the time to 5% white-rust coverage is 96 h for chrome-free self-lubricating SL2 and 48 h for chromate passivation C and inorganic chrome-free passivation IC — a factor of 2. Two boundaries belong on the process sheet: first, a passivated surface is unfavorable to the phosphating, ceramic conversion, chromating and spray painting that follow; second, the oil film must be removed with a cleaner that does not attack the coating, because strong alkaline or strong acid degreasing changes the surface chemistry of the coating. Fabrication scratches shorten life as well: published data give a Vickers hardness of about 140–160 HV for Zn-Al-Mg coatings and about 55–65 HV for pure zinc (other sources quote 40–160 HV, so rely on the mill certificate and your own measurement); scratch tests used a sapphire needle with a tip radius of 0.05 mm over a 20 mm stroke at loads of 0.0196–0.196 N, and the load at which a Zn-Al-Mg coating is scratched through is about 1.5 times or more that of Zn-5%Al and 3 times or more that of pure zinc and 55%Al-Zn.
Limits of a duplex system: residual passivation film, zinc soap and where the gain comes from
A duplex system — coating plus paint — usually outlives the two layers taken separately added together, but on Zn-Al-Mg the size of that gain is decided by the state of the interface. Three risks drive it: a residual passivation or anti-fingerprint film that bonds the paint to an organic layer rather than to metal; a zinc soap weak boundary layer that turns the interface into loose soluble salt under damp heat; and the pretreatment itself, which changes the surface chemistry of the coating, alkaline degreasing dissolving aluminum selectively. The line of reasoning for pure zinc parts is set out in more detail on our site, see Pretreatment before painting galvanized steel: zinc soap, white rust and duplex adhesion. The difference on Zn-Al-Mg is that MgZn2 in the eutectic region dissolves first and aluminum follows, so the interfacial chemistry moves faster, and the pretreatment parameters used for pure zinc parts cannot simply be copied across.
7.1 The old zinc-soap problem still applies to Zn-Al-Mg
The XPS interface work gives the mechanism used in failure analysis: adhesion of paint to a zinc coating is predominantly physical; under accelerated ageing soluble zinc corrosion products form at the interface, alkyd-type resins are saponified by zinc ions, and the resulting zinc soap weak boundary layer breaks adhesion (published research basis). The same logic holds on Zn-Al-Mg, only with more sources of soluble ions. Systematic testing of organic coatings on Zn-Al-Mg quantifies the relationship: Prosek et al. compared laboratory-painted cut edges on Zn-15Mg and Zn-1.5Al-1.5Mg across a series of accelerated tests (Progress in Organic Coatings 2015, 83: 26) and found that both delamination of the paint and red rust at the cut were smaller than on hot-dip galvanized steel of the same coating thickness in most conditions; Zn-15Mg performed better in the accelerated tests, but at the marine exposure site Zn-1.5Al-1.5Mg did better, which the authors attribute to the accumulation of low-solubility magnesium-bearing products. The same paper notes that the largest improvements appear under sustained high humidity, elevated temperature, high chloride load and where sulfate replaces chloride. For adhesive bonding, published patent US20190105889A1 describes a metal sheet assembly built as 'Zn-Al-Mg coating plus acid treatment plus adhesive'. The recent advance in interfacial chemistry is that surface hydroxylation affects the moisture durability of bonds to Zn, Zn-Al and Zn-Al-Mg coatings differently; that work was carried out by universities together with Baoshan Iron & Steel Co., Ltd. and other institutions (International Journal of Adhesion and Adhesives 2026, 10.1016/j.ijadhadh.2026.104299).
Translated into shop steps, the conclusions above become 'degrease — key — compatibility panel'. Work on zirconium conversion coatings (Surface and Coatings Technology 2020, 10.1016/j.surfcoat.2020.126236, from PSL, the Institut de la Corrosion in France and other institutions) monitored the in-situ reactions in a two-step sequence: the alkaline pretreatment removes the initial oxides and dissolves Al selectively, which limits the metal surface available for the subsequent fluorozirconate film to grow on; the same study reports that Cu²⁺ and NO₃⁻ markedly accelerate that process, so impurity ions in the degreasing bath are not a detail. Research on adhesion and corrosion disbondment of epoxy films on chemically etched ZnMgAl sheet likewise treats the effect of the alkaline step and the acid step on surface chemistry as the main variable. Engineering meaning: residual passivation and anti-fingerprint films are hidden interface layers inside the coating system — either use a primer compatible with them or remove them, and the phrase 'it sticks' is not a substitute for a compatibility panel. Primer selection is worked through on our pages Adhesion problems when painting aluminum, galvanized steel and stainless steel, and primer systems and Stopping paint peeling on galvanized steel and stainless steel: epoxy primer application guide.
| Pretreatment route | Interface behavior | Main risk | Quantified acceptance criterion |
|---|---|---|---|
| Direct painting over passivation or anti-fingerprint film | Paint bonded to an organic or conversion film rather than to metal | Adhesion rides on the cohesive strength of that film and decays after damp heat | Pull-off adhesion plus cross-cut grade measured together, with records kept |
| Alkaline degreasing | Removes the initial oxides and dissolves Al selectively | Less accessible metal area, uneven zirconium or silane film | Bath impurity ions and temperature under control, with a reference panel |
| Acidic activation or light etching | Activates the Zn-rich phase, eutectic regions respond first | Over-etching brings hydrogen embrittlement risk and white-rust residue | Time and temperature controlled, residue rinsed out completely and dried |
| Zirconium or silane conversion coating | Forms a nanometer-scale transition layer | Impurities such as Cu²⁺ and NO₃⁻ accelerate side reactions | Spot checks of coating weight or thickness plus adhesion re-test |
| Light keying (surface texturing) | Raises mechanical anchoring while keeping the coating | Over-strong parameters thin the coating or embed abrasive | Coating retention, no exposed steel, controlled roughness increase |
| St3 power-tool cleaning (local repair) | Cleaned back to a sound layer, white rust and scale removed | Incomplete feathering creates a new crevice starting point | Visual grading plus a record of the edge transition width |

The three-step pretreatment and the working limits of surface preparation grades
The working limits of a surface preparation grade are set by two rules: do not damage the coating, and do not introduce soluble salt. Zn-Al-Mg is a functional coating measured in the 20–35 µm range and is itself part of the corrosion protection; carrying over the blast parameters developed for bare steel to reach Sa2.5 will thin the coating or strip it in sheets and will embed abrasive in the soft zinc. The defensible approach, where mechanical anchoring is needed, is light keying at low abrasive hardness and low pressure (surface texturing), limited by 'coating retained, no exposed steel, controlled roughness increase'. Where bare steel really is required, restore potential and thickness with a thermal-sprayed zinc-aluminum metallic coating, an approach set out on our page Thermally sprayed zinc-aluminum metallic coatings: cathodic protection mechanism and ISO systems. Power-tool cleaning to St3 is safer for local repair, but it must go down to a sound layer and remove all white rust and scale. Soluble salt has to be accepted against a number: run the Bresle soluble-salt test with sampling per ISO 8502-6 and evaluation per ISO 8502-9, and at C3 and below keep chloride in the low-load class before painting. Blast roughness and grade assessment are covered on our page Surface preparation for industrial coatings: Sa2.5 blasting, roughness and dew point control, and the judgment of a rusty substrate plus the conversion pre-step on Surface preparation for painting over rust: St2/St3 cleaning, rust layer judgment and conversion pre-treatment.
8.1 Nominal dry film thickness, corrosivity category and re-inspection metrics
Nominal dry film thickness (NDFT) on a coated substrate must say whose thickness is meant: the total dry film of the paint system, or the combined film of coating plus paint. The systems listed in ISO 12944-5:2019 are informative examples, not a mandatory recipe; selection turns on substrate type, its initial condition, the surface preparation that is actually feasible, the corrosivity category, the durability sought, access for application and maintenance, and the measured record of the system itself. That part does not include CX or Im4 systems; offshore and extreme environments move to ISO 12944-9:2018, and the scheme for marine heavy-duty protection is on our page Offshore C5-M coating systems: salt spray, ultraviolet exposure and biofouling. Years do not belong in an acceptance clause: ISO 12944-1:2017 splits durability to first major maintenance into L (up to 7 years), M (7–15 years), H (15–25 years) and VH (more than 25 years) and states explicitly that durability is not a warranty period, which comes from the contract and is usually shorter. Write the re-inspection as three measurable items: pull-off adhesion per ISO 4624 or GB/T 5210, cross-cut per ISO 2409 or GB/T 9286, and accelerated ageing as NSS per GB/T 10125-2021 (NaCl 50 g/L ±5 g/L, 35 ℃, pH 6.5–7.2, fallout rate 1.0–2.0 mL/(80 cm²·h), recommended durations including 24, 48, 96, 168, 240, 480, 720 and 1008 h), with acceptance stated as creep of corrosion from the scribe and blistering grade rather than as 'so many years without rust'.
Application comparison and common specification errors
The same Zn-Al-Mg sheet behaves very differently across duties, and the most common specification error is to select an outdoor structural part as if it were an indoor appliance part. Solar mounting structures and frames, ductwork and cable tray corrode from punched and sheared edges, and the coating designation, sheet thickness and hole-to-edge distance together set the area ratio. Roof and wall cladding is dominated by seamed joints and screw nodes, where the risk is water held in laps and coating scratched during forming. Appliance backs and internal parts sit in dry indoor service, where appearance, earthing and anti-fingerprint performance are the asks. Automotive body and chassis parts see damp heat and de-icing salt, but they are qualified by the vehicle maker's cyclic corrosion program, so outdoor service years from the building-products side cannot be quoted for them. Poultry and livestock houses and fertilizer stores are defined by ammonia and acid deposition, and published supplier material states that Zn-Al-Mg resists ammonia better than pure zinc. The comparison is in the table below; the specification tier is set by corrosivity category and area ratio together.
| Application | Corrosion start and main exposure | Typical coating designation range | Does the cut edge need treatment | Common specification error |
|---|---|---|---|---|
| Solar mounting structures and frames | Punched edges and site-cut ends, mostly C2–C4 | ZM120–ZM310 | Small holes self-heal reliably; site-cut ends should be sealed | Specifying a low designation with thick plate as if it were an appliance part |
| Ductwork and cable tray | Seamed crevices, water retention and dust deposits | ZM120–ZM250 | Touch-up needed where drainage is poor | Comparing coating mass only and ignoring crevice geometry |
| Roof and wall cladding | Screw nodes and lap edges, strong orientation effects | ZM250 and above | End caps plus gasketed screws treated as one set | Inferring node life from flat-panel salt-spray results |
| Appliance backs and internal parts | Dry indoor service, appearance and earthing requirements | ZM120 grade with anti-fingerprint | Mostly internal parts, so appearance is the priority | Importing outdoor structural demands onto a low designation |
| Automotive body and chassis parts | De-icing salt, wet-dry cycling and stone chippage | Low-aluminum low-magnesium route | Weld and cut edges repaired to the vehicle specification | Quoting building-products outdoor years for a whole vehicle |
| Livestock houses and fertilizer stores | Ammonia, acid deposition and sustained high humidity | ZM250–ZM430 | Full scheme recommended in high-humidity zones | Grading the site as an ordinary industrial shed environment |
Failure-mode checklist and dissimilar-metal contact
Freezing the failure modes you can observe on site avoids the 'see rust, change material' reflex. One: red rust creeping from the cut edge, where an uncapped end face washed repeatedly by rain loses product as fast as it forms it, so the repair rate cannot catch up with the corrosion rate. Two: blistering and disbondment at the interface under the coating, usually traceable to residual passivation film, white rust left in place or soluble salt above the limit. Three: condensation during storage after coating that shows up later as adhesion failure — parts pass factory inspection and then lose paint in batches after coating. Four: galvanic coupling with a dissimilar metal, where direct contact with aluminum parts or stainless fasteners drives coating consumption through the potential difference and the area ratio; isolation and edge sealing are covered on our page Galvanic corrosion in steel-aluminum vehicle bodies: coating isolation, edge sealing and protective design. Five: coating spalling from forming and die build-up, concentrated where bend and flange radii are too small. Six: local attack where the steel touches concrete or chloride-bearing insulation and inside water-holding crevices — a crevice-corrosion duty that calls for isolation and drainage, not a thicker coat of paint.
Repaint and repair boundaries: when stripping to bare metal is not required
Repainting an old Zn-Al-Mg member does not automatically mean stripping the whole thing to bare metal, but three questions must be answered first: how far the rusting has gone, whether soluble salt is above the limit, and whether the passivation or anti-fingerprint film is still there. Full blasting to Sa2.5 thins the coating and embeds abrasive, and it is only worth doing where the coating has been substantially consumed, the paint is disbonding over large areas, or pitting has perforated the section; otherwise take the route of 'clean back to a stable interface, feather the edges locally, compatible primer, matched finish coat' — the grading of rust and rusty substrate is on our page Surface preparation for painting over rust: St2/St3 cleaning, rust layer judgment and conversion pre-treatment. For roof-type members, the line of rust grading, surface preparation grade and specified film thickness has its own page at Repainting color-coated steel roofs: rust grading, surface preparation grade and specified film thickness; this one deals only with the interface and cut-edge issues specific to a ternary coating.
10.1 Coating choice for local touch-up
The order of work for ends and drilled holes: deburr mechanically and degrease to remove salt, then apply a zinc-rich or zinc-aluminum repair coating over the exposed steel, then fit end caps or seal the end face so that direct rain and dust accumulation are kept off and the product film has stable conditions in which to form — painting without sealing simply washes off, and sealing without painting lets the bare face rust as before. Solids content and film thickness of the repair coating follow the supplier's technical data sheet; check them on site with a magnetic or eddy-current thickness gauge and keep the record. Adhesion differences and application notes for epoxy primers on galvanized steel, aluminum and stainless steel are on our page Stopping paint peeling on galvanized steel and stainless steel: epoxy primer application guide. If the member has to be welded, the coating in the heat-affected zone has been metallurgically changed, so repair it with a zinc-aluminum coating and re-check adhesion rather than assuming the weld zone still has its original coating capability.
Key figures (every item carries its unit)
- EN 10346:2015 requirement for a ZM bath: aluminum plus magnesium totaling 1.5%–8%, magnesium not less than 0.2%, balance zinc, with the applicable thickness written as 0.20 mm ≤ t < 3.0 mm.
- Version timeline: the DIN draft of 2025-06 and BS EN 10346:2026 (published 2026-10-28) extend the thickness range to 0.20 mm–6.5 mm and add designation A for pure aluminum coating.
- GB/T 2518-2019 was published 2019-12-10 and implemented 2020-07-01, covers 0.20 mm–6.0 mm, supersedes GB/T 2518-2008 and GB/T 14978-2008, and designates four coating types: Z, ZF, ZA and AZ.
- Coating designations and masses reproduced from GB/T 31447-2015: YZ (99.9% Zn) averaging 600 g/m², i.e. 84 µm; YZM (Zn-0.5% Mg) averaging 225 g/m², i.e. 32 µm; YZAM (Zn-11% Al-3% Mg-0.2% Si) averaging 138 g/m², i.e. 25 µm.
- GB/T 18226-2025 was published 2025-08-29 and implemented 2026-03-01 and, according to published data, introduces a Zn-Al-Mg alloy coating clause; the hot-dip galvanizing average coating mass lines are 600 g/m² for main structural members and 350 g/m² for fasteners, and hot-dip galvanizing plus powder coating is zinc 275 g/m² with 76 µm of polymer.
- Critical cut-edge to coating area ratio 0.5; conversions: t divided by twice the ring width for an annulus, 2t/L for a square panel; 1.5 mm plate with a 10 mm supply band gives 0.075.
- Mean cut-edge mass-loss rate after 24 h neutral salt spray: 0.0104 for pure Zn, 0.00988 for Zn-Mg, 0.00573 for Zn-Al and 0.00521 g/(m·h) for Zn-Al-Mg, the two aluminum-bearing coatings at roughly half the rate of pure zinc (Journal of the Chinese Society for Corrosion and Protection, 2026, 46(3): 703).
- Height difference between cut-edge steel substrate and coating after 6 h immersion in 5% NaCl: 9.7, 6.2, 5.7 and 5.1 µm; cut-edge resistance ranks Zn-Al-Mg above Zn-Al, and both above Zn-Mg and pure Zn.
- ISO 9223 first-year thickness loss for zinc: C1 not exceeding 0.1, C2 0.1–0.7, C3 0.7–2.1, C4 2.1–4.2, C5 4.2–8.4 and CX 8.4–25 µm/a.
- NSS parameters in GB/T 10125-2021 and ISO 9227:2017: NaCl 50 g/L ±5 g/L, 35 ℃, pH 6.5–7.2, fallout rate 1.0–2.0 mL/(80 cm²·h), recommended durations up to 1008 h; the standards state explicitly that salt spray is not used for ranking corrosion resistance or predicting service life.
Frequently asked questions
How far can a Zn-Al-Mg cut edge actually self-heal?
The auditable criterion is an area ratio rather than a fixed radius. The published test laser-cut annular specimens and varied the ratio of cut-edge area to coating area: resistance to red rust was good below 0.5, and the red-rust area grew as the ratio rose. Converted here, a ring gives roughly t divided by twice the ring width and a square panel gives 2t/L, so thick plate, small parts, densely spaced large holes and site thermal cutting are high-risk geometries that need edge protection by sealing or touch-up instead of reliance on the material to close the gap.
After site flame or plasma cutting, must the end face be painted?
Treat it as mandatory. A thermally cut face carries an oxide layer, dross and micro-cracks and is far rougher than a factory punched face, so a continuous protective film struggles to form while rain, dust and salt accumulate on it. Cut ends also sit where water and dew collect. The workable sequence is to remove dross and burr mechanically, degrease and desalinate, apply a zinc-rich or zinc-aluminum repair coating over the exposed steel, then fit an end cap or seal the face so direct rain is kept out and the product film can form under stable conditions.
Is ZM310 a thicker coating than Z275, and can g/m² be compared directly?
Not directly. The designation gives the total coating mass on both sides, so it has to be converted to per-side thickness: Z275 works out to about 20 µm per side at the pure zinc density of roughly 7.1 g/cm³, while Zn-Al-Mg is slightly less dense and published data put ZM120, ZM250, ZM310 and ZM430 at about 10, 20, 25 and 35 µm per side. ZM310 is therefore thicker per side than Z275, but cross-system price comparison and acceptance should be written in per-side thickness or as designation plus mill certificate, otherwise an order placed on coating mass can arrive with a thinner film than intended.
Can you spray paint straight onto Zn-Al-Mg sheet, and what about the residual passivation film?
Read the mill's surface post-treatment code first. Surfaces that have received chromate or chrome-free passivation are unfavorable to phosphating, ceramic conversion and painting, and any oil film must be removed with a cleaner that does not damage the coating. The workable route is the three steps of degreasing, keying and a compatibility panel: watch for selective dissolution of aluminum during alkaline degreasing, keep keying below the point where the coating is damaged, and release volume work only after the panel passes both pull-off adhesion and cross-cut. A residual film is either bridged by a compatible primer or removed outright; it is not a matter of judging by feel whether it will hold.
Can Sa2.5 be used on Zn-Al-Mg parts, and how far is safe?
Blasting bare-steel parameters straight across will thin or strip the functional coating measured in the 20–35 µm range and embed abrasive in soft zinc. The engineering rule is light keying limited by 'do not damage the coating, do not introduce soluble salt', accepted on three items: coating retention, no exposed steel, and a controlled roughness increase. Where bare steel is genuinely required, restore potential and thickness with a thermal-sprayed zinc-aluminum metallic coating and then build the scheme per the ISO 12944 series. For local repair prefer St3, taken back to a sound layer with all white rust and scale removed.
There is white rust on the sheet — is it still usable, and does it affect the paint work?
First tell white rust from red rust. White rust is the corrosion product of zinc formed under a water film, a white to gray powder, usually caused by package condensation, water ingress or poor stack ventilation; published data give the sensitive range as relative humidity near 60% and 85%–95%, water-film pH below 6 and about 70 ℃. Light white rust can be cleaned and re-inspected, but it is a loose, water-bearing interface with unstable conductivity, so painting over it loses adhesion after damp-heat cycling. Remove the product, check soluble salt with the Bresle test sampled per ISO 8502-6 and evaluated per ISO 8502-9, then set the primer and the film thickness.
What isolation is needed where the part touches aluminum or stainless steel fasteners directly?
Establish first that the coating protects the steel sacrificially: published data put the electrode potential of zinc near −0.76 V and iron near −0.44 V, and Zn-Al-Mg coatings work by the same sacrificial-anode mechanism. Direct contact with aluminum or stainless steel lets the potential difference and the exposed area ratio accelerate coating consumption, and water held in the crevice confines the attack to the contact face. Use either an insulating scheme or a potential-matched one, add washers and sealant, avoid geometry that stores water, and seal cut edges and drilled holes. Our article on galvanic corrosion in steel-aluminum vehicle bodies covers isolation and edge sealing in more depth.
The supplier claims '10 times the corrosion resistance of pure zinc' and '30 years without rust'. How should the acceptance clause read?
Treat multiples as screening information and write only measurable items into the clause. The salt-spray method standards themselves state that the test is not applicable to ranking the corrosion resistance of different materials and cannot predict service life — GB/T 10125-2021 and ISO 9227:2017 both say so — and supplier multiples usually come from one alloy route, one specimen condition and one test cycle. Write in: coating designation and per-side thickness with the mill certificate, corrosivity category and ISO 12944 system tier, nominal dry film thickness, a soluble-salt limit, adhesion and scribe-creep criteria, plus the re-inspection sampling ratio and the test-method standard numbers, so that every term is measurable and reproducible.
References and basis of the figures used
Every figure in this article comes from published standards, journal literature and suppliers' public documentation. Items marked 'published-data basis' or 'supplier data' have not been verified by a third party and must not be used directly as contract acceptance criteria; standard text is governed by the official document and journal data by the original paper. This article is written on a B2B technical basis, and the foreign-trade terms discussed are EXW and FOB only.
Last updated: 2026-11-12. Prepared by the technical team of Kexin New Materials (Guangdong) Co., Ltd. from published standards and literature, as a reference for industrial coating selection and failure analysis. It is not a guarantee of the service life of any specific component.